| HS Code | 776322 |
| Filler Type | Mineral |
| Filler Content | 20% |
| Density | 1.04 g/cm³ |
| Melt Flow Rate | 10 g/10 min |
| Tensile Strength | 25 MPa |
| Tensile Elongation At Break | 20% |
| Flexural Modulus | 2200 MPa |
| Notched Izod Impact Strength | 4 kJ/m² |
| Heat Deflection Temperature At 1 82 Mpa | 100 °C |
| Vicat Softening Temperature | 150 °C |
| Mold Shrinkage | 1.0-1.4% |
| Flame Rating | HB |
| Water Absorption | <0.02% |
| Processing Method | Injection Molding |
As an accredited Kingfa PP-KF06,PP-TD20,Mineral Filled, Automotive/Appliance factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Kingfa PP-KF06 PP-TD20 mineral-filled polypropylene resin for automotive/appliance parts, supplied in 25 kg moisture-resistant bags. |
| Container Loading (20′ FCL) | Kingfa PP-KF06 (PP-TD20 mineral-filled polypropylene for automotive/appliance) is palletized and securely loaded into a 20′ FCL container for export. |
| Shipping | Shipping description: Kingfa PP-KF06 (PP-TD20) mineral-filled polypropylene is typically shipped as dry pellets in sealed 25 kg bags or bulk containers. It is non-hazardous and not regulated for transport; no UN number, hazard class, or special label is required. Store away from moisture and direct sunlight. |
| Storage | Store Kingfa PP-KF06, PP-TD20 mineral-filled polypropylene in a cool, dry, well-ventilated area away from direct sunlight, heat, ignition sources, and incompatible chemicals. Keep in original sealed packaging to prevent moisture and contamination. Maintain stable ambient temperature; avoid humid, dusty conditions and prolonged outdoor exposure. Use first-in, first-out inventory. Handle with normal industrial hygiene and minimize dust generation during transfer. |
| Shelf Life | Kingfa PP-KF06 has a typical shelf life of 24 months when stored cool, dry, and in original unopened packaging. |
Kingfa PP-KF06 and PP-TD20 are mineral-modified polypropylene injection molding grades with nominal filler loading in the 20 wt% range. Published third-party data for these specific Kingfa designations is limited; the following application scenarios therefore reference process windows and performance limits representative of 20% mineral-filled PP compounds, with grade-specific validation required under ISO 11469. The application split is not arbitrary. PP-KF06 is typically deployed where high melt flow, thin-wall fill, and low warpage dominate, while PP-TD20 is specified where impact energy, structural creep recovery, and long-flow flatness are more critical.
| Application track | Grade | Flammability | Emissions or weathering | Mechanical | Dimensional |
|---|---|---|---|---|---|
| Automotive interior trim | PP-KF06 | ISO 3795 | VDA 277, VDA 270, ISO 6452 | ISO 527-2, ISO 178, ISO 179-1/1eA | ISO 294-4 |
| Automotive HVAC ducts | PP-KF06 | UL 94 HB at 1.6 mm | VDA 278 | ISO 527-2, ISO 179-1/1eA | ISO 294-4 |
| Appliance housings | PP-TD20 | IEC 60695-11-10, IEC 60695-2-11 750 °C | Not required | ISO 179-1/1eA | ISO 294-4 |
| Washing machine tubs | PP-TD20 | IEC 60335-1 clause 30.2 | Not required | ISO 527-2, ISO 179-1/1eA | ISO 294-4 |
| Semi-exterior cowl grille | PP-TD20 | ISO 3795 | SAE J2527 | ISO 179-1/1eA at -30 °C | ISO 294-4 |
In thin-wall automotive interior trim, the dominant failure modes are short shots, visible flow hesitation marks, and post-mold warpage caused by anisotropic shrinkage. PP-KF06 is assigned to A/B/C pillar trim covers, rear side trim, and seat side shields because its mineral filler reduces longitudinal mold shrinkage to below 1.3% and improves flatness over unfilled PP. Injection is typically performed on hydraulic toggle presses with clamp force between 3,500 kN and 6,000 kN, using a general-purpose polyolefin screw with L/D ratio 20:1–24:1 and compression ratio 2.2:1–2.8:1. Melt temperature is held at 220–240 °C, while mold temperature is set at 30–50 °C to balance cycle time against grain retention and dimensional stability. For wall sections below 2.0 mm, fill time should not exceed 1.0 s, and screw advance velocity is raised until cavity pressure rise occurs after the flow front has passed the last visible surface. Hold pressure is staged from 50 MPa down to 20 MPa over 6–8 s to minimize gate sink and to maintain clamp force margins. The material is not pre-dried unless storage has exceeded 8 h at relative humidity above 60%, in which case 80 °C for 2 h in a desiccant dryer prevents splay. Compliance for interior trim is governed by ISO 3795 for horizontal burning rate, ISO 6452 for fogging mass and reflectance, VDA 277 for total volatile organic compound emissions, and VDA 270 for odor rating. OEM-level specifications frequently add fogging condensate limits below 2 mg and total VOC limits below 50 µgC/g, although exact threshold values are part-specific and must be retrieved from the relevant engineering standard. Finished parts include demister adapters, lower door panel inserts, and rear parcel shelf supports. PP-KF06 is not recommended for upper surface parts subjected to continuous direct solar load because the heat deflection temperature of 20% talc-filled PP under 0.45 MPa load is typically below 115 °C, and creep can accumulate in dark-colored skins at stagnant cabin temperatures above 85 °C.
For air purifier base housings, dehumidifier fan support brackets, and floor cleaner wheel covers, PP-TD20 is used because the loading includes low-speed impact, stacking compression, and continuous vibration from small AC or BLDC motors. The mineral filler supplies flatness across large rectangular sealing faces, while the impact modification prevents brittle fracture at snap-fit tabs during service assembly. Molding is performed with sequential valve-gated hot runners to avoid weld lines around the fan outlet annulus; gate positions are selected so that flow fronts meet at non-appearance rib intersections rather than at sealing ribs. Melt temperature is set at 230–250 °C, mold temperature at 40–60 °C, and pack pressure is maintained long enough to prevent warpage after demolding. Regrind from sprues and runners is limited to 15–20 wt% for internal parts because higher regrind fractions alter color and reduce impact reproducibility in mineral-filled PP. Flammability is assessed under IEC 60695-11-10 for UL 94 HB at 1.6 mm, and glow wire testing under IEC 60695-2-11 at 750 °C is required for unattended appliance housings in accordance with IEC 60335-1 clause 30.2. Electrical safety, creepage distance, and clearance design are governed by IEC 60335-1 clause 29, but the material itself is used as an insulator only in non-primary isolation areas. RoHS directive 2011/65/EU and REACH Article 33 notification obligations apply to the finished article. Terminal components include air purifier front frames, dehumidifier water tank brackets, and robot vacuum dustbin housings.
Washing machine outer tubs and balance rings molded from PP-TD20 require a different process logic than thin-wall trim because the dominant risks are cavity-to-cavity fill imbalance, weld line failure near the bearing housing, and post-mold ovality from differential crystallinity. The tub is typically molded in two halves on large injection units with shot capacity above 5 kg, using multiple sequentially opened valve gates. Melt temperature is maintained at 230–250 °C, mold temperature at 40–60 °C, and the hold pressure profile is extended over the gate seal time to compensate for mold shrinkage of 1.0–1.5%. Weld lines are placed away from the bearing boss and drain port because weld factor in mineral-filled PP can reduce notched impact strength relative to un-welded material; reductions of 20–40% have been reported in talc-filled PP literature, but production tools require direct weld line Charpy measurement rather than reliance on literature values. Balance ring sections are molded as upper and lower shells, then friction welded or hot-plate welded; the weld joint must remain leaktight at the appliance maximum spin speed under a water-loaded drum. Detergent resistance is verified by immersion in water at 60–90 °C with alkaline detergent concentration corresponding to wash cycles, followed by ISO 527-2 tensile strength retention. Dimensional stability after aging is assessed according to ISO 294-4 shrinkage data, and impact strength is measured under ISO 179-1/1eA at 23 °C and -10 °C. Regulatory compliance follows IEC 60335-1 clause 22.6 for drainage, clause 30.2 for glow wire, and EU 2019/2021 ecodesign provisions for dynamic spin stability where appliance-level testing applies. Published data for this specific PP-TD20 configuration in washing machine tubs is limited, so tool trials with gate sequencing and counterpressure optimization are required before production release.
Automotive HVAC distribution ducts and defroster nozzle assemblies operate under cyclic air temperatures from -30 °C to 90 °C, with low structural load but strict dimensional tolerance for sealing and clip retention. PP-KF06 is injection molded into duct halves with wall thickness from 1.5 mm to 2.5 mm, using collapsible cores or mechanically actuated slides for undercut snap features. The high melt flow allows fill length-to-wall thickness ratios above 120:1, but gate location must avoid the visible outlet edge where flow hesitation creates V-shaped ghost marks. Melt temperature is set at 220–240 °C and mold temperature at 30–50 °C. Warpage is controlled by maintaining uniform 20 wt% filler dispersion and by avoiding abrupt wall thickness changes above 15% at gusset bases. Emissions are tested via VDA 278 thermal desorption with VOC and fogging components; ISO 6452 photometric fogging is also applied to glazing protection. Flammability classification is usually UL 94 HB at 1.6 mm. Finished components include floor outlet ducts, demister nozzles, and vent adapters. The grade is not suited to engine compartment hot-side ducts where continuous air temperatures above 110 °C can exceed the heat deflection limit of talc-filled PP.
When PP-KF06 is selected as a replacement for ABS in rice cooker side frames, water dispenser front panels, and soy milk maker motor mounts, the design must compensate for lower tensile modulus and higher shrinkage anisotropy. ABS typically exhibits mold shrinkage of 0.4–0.7%, while 20% talc-filled PP exhibits 0.9–1.3% along flow and 1.1–1.5% transverse. Rib-to-wall ratios are therefore held at 50–60% to prevent sink marks on visible surfaces, and bosses are redesigned with outer diameter 2.0–2.5 times the screw diameter. Processing energy is reduced because melt temperature is 220–240 °C compared with ABS at 230–260 °C, and mold temperature can be lowered from 60–80 °C to 30–50 °C. The material is pre-dried at 80 °C for 2 h only when exposure to humid air exceeds 8 h. Surface finish is limited to matte or textured grain; high-gloss piano-black surfaces are not suitable without painting or film lamination. For chemical exposure to steam, citric acid, and detergent residues, PP offers stress-cracking resistance superior to ABS, but creep resistance at temperatures above 80 °C is lower. Snap-fit assembly requires larger insertion angles and lower interference because notched impact strength of talc-filled PP drops at high strain rates. Underwriters Laboratories HB classification is tested at 1.6 mm, and household appliance housing standards IEC 60335-1 clause 30.2 apply to glow wire resistance. Terminal parts include small appliance motor brackets, control panel backing frames, and hinge supports.
Cowl grille panels and wiper motor covers occupy a semi-exterior zone where the polymer sees intermittent engine heat, road splash, windshield washer fluid, and solar UV, but not Class A paint requirements. PP-TD20 is compounded with UV stabilizers and carbon black to retain surface integrity under SAE J2527 exposure at 1,250 kJ/m² at 0.55 W/m² irradiance without significant graying or chalking. The injection mold is textured with grain depth 15–25 µm to hide flow lines and mineral flake orientation. Melt temperature is 230–250 °C, mold temperature 30–60 °C, and the part is cooled on a jig after demolding to avoid edge curl along the windshield interface. Dimensional tolerance for the wiper spindle opening is held by controlling mold shrinkage to 1.0–1.4% and by measuring ISO 294-4 shrinkage panels from each lot. Low-temperature impact is evaluated under ISO 179-1/1eA at -30 °C because stone impact and snow brush loading can initiate brittle fracture at subfreezing conditions. Drainage slots and water channels are designed with draft angles above 1.5° to allow demolding against grain. Terminal components include cowl grille assemblies, wiper motor covers, and wiper arm trim caps. This grade is not specified for structural cowl cross-members or for painted exterior body panels because mineral-filled PP has low surface energy and requires flame or corona treatment for durable coating adhesion.
Air-conditioner drain pans and cross-flow fan scroll housings impose simultaneous requirements for condensate containment, vibration damping, and flatness over long sealing faces. PP-TD20 is evaluated for these parts because the mineral filler raises tensile modulus and reduces creep, while the impact modification resists crack propagation from fan imbalance or shipping loads. The drain pan is injection molded with wall thickness 2.0–3.0 mm, and flatness across a 500 mm diagonal is controlled to better than 1.0 mm by optimizing gate locations and using a cooling fixture after ejection. Melt temperature is set at 230–250 °C, mold temperature at 40–60 °C, and injection velocity is reduced near the end of fill to avoid gas entrapment at the drain outlet boss. Fastener bosses are designed with outer diameter 2.0–2.5 times the screw major diameter and ribbed gussets to distribute hoop stress. Condensate exposure testing is performed with water at 5 °C to 60 °C under thermal cycling, followed by ISO 527-2 tensile retention. Microbial growth is not a material property but is mitigated by smooth mold surfaces with SPI A-2 finish or better. Flammability is evaluated under UL 94 HB at 1.6 mm, and glow wire testing under IEC 60695-2-11 at 650 °C or 750 °C is applied depending on appliance location and accessibility. The cross-flow fan scroll housing is often molded in two halves and assembled by snap-fit or screws; weld lines at the scroll tongue must be moved away from the high-velocity outlet because turbulent pressure pulsation accelerates fatigue crack growth. Terminal parts include indoor unit drain pans, outdoor unit fan scrolls, and air guide louvers. PP-TD20 is not specified for compressor base plates or high-temperature gas-side components because creep and temperature limits of 20% mineral-filled PP are insufficient above 90 °C under continuous mechanical load.
Competitive Kingfa PP-KF06,PP-TD20,Mineral Filled, Automotive/Appliance prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8615365186327 or mail to sales3@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8615365186327
Email: sales3@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Kingfa PP-KF06 and PP-TD20 are mineral-filled polypropylene compounds positioned for injection-moulded automotive and appliance components. The two grade designations are read as separate model suffixes within the supplier’s PP portfolio: PP-TD20 is consistent with a nominal 20 wt% talc-filled polypropylene, while PP-KF06 belongs to a mineral-filled flow-modified family whose exact filler chemistry is not fully disclosed in public literature. Under ISO 1043-1 and ISO 11469, the materials would be marked as discrete mineral-filled PP designations, although the exact marking code for the specific talc or mineral content must be confirmed from the supplier certificate. Published public datasheet values for these exact Kingfa suffix codes are limited; therefore, numerical intervals in this page are reference profiles for talc-filled or mineral-filled PP according to the cited standard methods, not guaranteed lot values. The intended use is high-volume injection moulding where dimensional stability, stiffness, and short-term thermal resistance are required, with automotive and appliance sectors governing most processing decisions.
Mineral-filled PP is not aggressively hygroscopic, but talc surfaces can retain atmospheric moisture. When granulate is stored at ambient relative humidity above 60% or transferred from an unheated warehouse into a warm production hall, predrying in a desiccant dryer at 80°C for 2 h to 3 h with a dew point not exceeding −20°C is used to prevent splay and melt-pressure oscillation. If granulate is supplied in sealed moisture-proof packaging and consumed within one shift at controlled humidity below 40%, drying may be omitted.
The injection-moulding melt temperature should remain between 210°C and 240°C; talc raises viscosity and shear heating. Barrel temperature zones from feed throat to nozzle are typically configured as 190°C, 200°C, 210°C, 220°C, and 230°C, but charge transition and screw recovery time provide better control than nominal set points. Mould surface temperature between 30°C and 60°C balances cycle time against weld-line strength and surface gloss. A general-purpose reciprocating screw with an L/D of 22:1 and a compression ratio of 2.5:1 to 3.0:1 is acceptable for these grades; back pressure of 3 bar to 8 bar and screw speed of 40 rpm to 80 rpm are class-typical starting points. Actual conditions must be established on the production tool because gate geometry, runner balance, and cooling-circuit layout override generic recommendations.
Compounding of these mineral-filled grades is typically performed on co-rotating twin-screw extruders with L/D 40:1; talc addition is split between the main feed and side feeder to limit screw torque and preserve coupling efficiency. Injection moulding downstream is on reciprocating-screw machines with clamp force matched to projected area so that cavity pressure does not exceed 50 MPa while avoiding flashing.
Rheological characterisation under ISO 1133-1:2022 at 230°C and 2.16 kg for a nominal 20 wt% talc-filled PP typically falls in the melt mass-flow rate range of 10 g/10 min to 20 g/10 min, while controlled-flow mineral-filled formulations for thin-wall work may extend to 25 g/10 min or higher. MFR is a low-shear index and does not replace capillary or in-line rheometry at injection shear rates of 103 s−1 to 104 s−1. When MFR exceeds 30 g/10 min, impact retention can drop below automotive interior trim requirements and flash may appear at vents or ejector clearances. When MFR falls below 8 g/10 min, short shots are more likely in parts with flow-length to wall-thickness ratios above 150:1. For these two Kingfa grades, the public MFR boundaries are not disclosed; the same physical thresholds apply to any mineral-filled PP at equivalent filler content.
On production-scale injection moulding machines with 1200 t clamp force or more, batch-to-batch drift in MFR of mineral-filled PP is conventionally held within ±10% of nominal for automotive grades; no public control limits are available for these two Kingfa suffixes. This drift influences screw recovery time, cushion control, and packing demand. When MFR drifts upward, cavity-pressure profiles show earlier gate freeze and lower pack effectiveness; when MFR drifts downward, peak injection pressure may exceed the machine pressure limit if the tool was not designed with pressure margin. Moulders therefore control these grades by cavity pressure rather than timer-based cut-off. Pressure at switch-over is typically 30 MPa to 50 MPa hydraulic or 200 bar to 400 bar specific injection pressure, but the actual limit is determined by melt compressibility and tool deflection.
PP-TD20 and PP-KF06 are not direct substitution grades. The TD20 suffix is read as a nominal 20 wt% talc-filled polypropylene with higher flexural modulus and lower mould shrinkage than unfilled PP, while KF06 is a mineral-filled formulation oriented toward controlled flow and dimensional consistency in complex tools. The exact filler chemistry of KF06 is not published in an open datasheet; published data for this specific configuration is limited. The practical selection difference for process engineers is not only filler content but also the interaction among flow length, packing hold time, and anisotropic shrinkage. A higher talc loading reduces notched impact and weld-line strength; a more flow-modified grade can improve fill but may exhibit lower low-temperature Charpy impact. Reference data in Table 1 are class-typical intervals for 20 wt% talc-filled PP based on ISO and UL methods; supplier certificate values for Kingfa PP-KF06 and PP-TD20 take precedence.
| Property | Standard method | Reference interval | Unit |
|---|---|---|---|
| Density | ISO 1183-1:2019 | 1.03–1.08 | g/cm³ |
| Melt mass-flow rate | ISO 1133-1:2022, 230°C/2.16 kg | 8–20 | g/10 min |
| Tensile stress at yield | ISO 527-2, type 1A, 50 mm/min | 24–30 | MPa |
| Tensile strain at yield | ISO 527-2, type 1A | 3.0–5.0 | % |
| Flexural modulus | ISO 178, 2 mm/min | 2300–3100 | MPa |
| Charpy notched impact, 23°C | ISO 179-1/1eA | 2.5–5.5 | kJ/m² |
| Charpy notched impact, −30°C | ISO 179-1/1eA | 1.5–3.0 | kJ/m² |
| Heat deflection temperature | ISO 75-2/B, 0.45 MPa | 95–120 | °C |
| Vicat softening temperature | ISO 306/A50 | 125–145 | °C |
| Mould shrinkage, flow | ISO 294-4 | 0.6–1.0 | % |
| Mould shrinkage, transverse | ISO 294-4 | 0.8–1.2 | % |
| Flammability | UL 94 / IEC 60695-11-10 | HB | class |
The observed processing difference on production equipment is often shrinkage anisotropy rather than absolute shrinkage. For a nominal 20 wt% talc-filled PP, flow-direction mould shrinkage is commonly 0.6% to 1.0% and transverse shrinkage is 0.8% to 1.2%; unfilled PP can exceed 1.5%, while 30 wt% glass-filled PP may drop below 0.4%. PP-KF06, when used for automotive interior substrates, is typically processed with comparable shrinkage but with narrower lot-to-lot control on the supplier certificate; however, published data for this specific configuration is limited. Weld-line tensile strength in talc-filled PP is often 30% to 45% lower than the un-welded base material under ISO 527-2, so moving cores or sequential valve gates are required in high-stress zones. Compared with 20 wt% glass-fiber-reinforced PP, the talc-filled grade generates lower warpage anisotropy, better surface finish, and less abrasive wear on mould steel, but lower tensile strength and notched impact.
In automotive execution, PP-TD20 and PP-KF06 are used in interior and exterior trim carriers, HVAC housings, battery trays, wheel-arch liners, and structural brackets where short-term thermal resistance up to 100°C is required. Interior material acceptance is conditioned by flammability testing under ISO 3795 or FMVSS 302; odour and emissions are measured under VDA 270 and VDA 278. Exterior trims require UV stabilization; talc-filled PP without light-stabilizer packages degrades under xenon-arc exposure, and accelerated weathering according to SAE J2527 or ISO 4892-2 must demonstrate ΔE and gloss retention within OEM limits. On production-scale injection lines, gate location and cooling uniformity control surface quality more than a nominal melt-flow number alone. Unbalanced hot-runner manifolds in multi-cavity tools can produce sink marks and gloss variation because mineral platelets orient parallel to flow near the gate. Packing pressure must be held until gate freeze; for talc-filled PP with a gate diameter of 1.0 mm to 1.5 mm, freeze time is commonly 2 s to 4 s at wall thickness 2.5 mm to 3.0 mm, but the actual value is set by gate steel conductivity and cooling-channel placement.
Mineral-filled PP responds to filler content increases by lowering mould shrinkage and thermal expansion while reducing notched impact resistance. For a nominal 20 wt% talc-filled PP, the coefficient of linear thermal expansion in the flow direction is typically 60 × 10−6 K−1 to 90 × 10−6 K−1 under ISO 11359-2, compared with 100 × 10−6 K−1 to 150 × 10−6 K−1 for unfilled PP. This reduction is exploited in appliance structural parts where mated clearances must survive thermal cycling. The trade-off is a reduction in Charpy notched impact and weld-line integrity: a class-typical 20 wt% talc-filled grade exhibits 2.5 kJ/m² to 5.5 kJ/m² at 23°C, which is below that of unfilled impact copolymers and well below that of 30 wt% glass-filled PP at equal wall thickness.
Appliance structural components such as washing-machine outer tubs, dishwasher bases, and microwave oven brackets use mineral-filled PP for resistance to alkaline detergents and hot water. Under IEC 60335-1:2020, heat resistance may be assessed by ball-pressure testing at 125°C; under IEC 60695-2-11, glow-wire ignition at 750°C may be required for unattended appliances. A 20 wt% talc-filled PP such as PP-TD20 can usually meet ball-pressure at 125°C, but it is not inherently UL 94 V-0; flame-retardant packages that achieve V-0 can reduce notched impact by 25% to 40% and produce acidic decomposition by-products during processing. Chemical resistance to 5 wt% sodium hydroxide solution at 80°C for 72 h is generally acceptable; however, published data for this specific Kingfa configuration is limited. For food-contact appliance parts, compliance must be verified under EU 10/2011 or FDA 21 CFR 177.1520, with mineral filler purity and processing-aid migration as the limiting parameters.
Compared with ABS, mineral-filled PP has lower density, lower emissions, and better fatigue resistance under repeated flexural load, but lower surface hardness and lower creep resistance above 90°C. Compared with 30 wt% glass-fiber-reinforced PP, the talc-filled grades provide lower warpage anisotropy and less audible noise radiation from integral mounts, while sacrificing tensile modulus and notched impact strength. These differences make PP-TD20 and PP-KF06 preferable for large-area thin-wall housings and thermally cycled brackets, provided that the tooling gate map and process window are qualified against the actual certificate values rather than the class-typical intervals shown here.