| HS Code | 330777 |
| Productname | Kingfa AIP-2015 |
| Materialtype | PP + EPDM + TD20 |
| Polymerbase | Polypropylene |
| Elastomer | EPDM |
| Filler | Talc |
| Fillercontent | 20% |
| Automotiveapplication | Interior/Dashboard |
| Density | 1.04 g/cm3 |
| Meltflowrate | 20 g/10 min (230 C/2.16 kg) |
| Tensilestrength | 18 MPa |
| Flexuralmodulus | 1500 MPa |
| Notchedcharpyimpactstrength | 10 kJ/m2 |
| Heatdeflectiontemperature | 100 C at 0.45 MPa |
| Moldingshrinkage | 1.0-1.4% |
| Processingmethod | Injection molding |
As an accredited Kingfa AIP-2015,PP+EPDM-TD20,Automotive, Interior/Dashboard factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Kingfa AIP-2015 PP+EPDM-TD20 automotive interior/dashboard pellets are packed in 25 kg moisture-proof bags, palletized and shrink-wrapped for shipment. |
| Container Loading (20′ FCL) | 20′ FCL dry container loaded with palletized, shrink-wrapped 25 kg bags of Kingfa AIP-2015 PP+EPDM-TD20 automotive interior/dashboard compound, securely stowed. |
| Shipping | Kingfa AIP-2015 (PP+EPDM-TD20), an automotive interior/dashboard thermoplastic compound, is shipped as non-hazardous pellets in sealed moisture-proof bags or octabins. Transport in clean, dry trucks/containers at ambient temperature, protected from direct sunlight, heat, moisture, and contamination. No dangerous-goods classification applies; use normal stacking and handling precautions. |
| Storage | Store in a cool, dry, well-ventilated area away from direct sunlight, heat sources, and moisture. Keep material in original sealed bags or containers on pallets, avoiding dust, oil, and other contamination. Do not stack excessively or expose to prolonged high temperatures. Maintain stable conditions and follow the supplier’s safety data sheet and shelf-life recommendations. |
| Shelf Life | Shelf life: typically 24 months from production date in original sealed packaging, stored dry, cool, ventilated, away from sunlight and moisture. |
In hard instrument panel carrier applications, Kingfa AIP-2015 is specified where the combined requirement is flexural modulus above 1,800 MPa, heat deflection under 0.45 MPa above 110 °C, and flame-spread compliance under FMVSS 302 or ISO 3795 without halogenated flame retardants. The governing combustion standard permits self-extinguishing burn rates not exceeding 100 mm/min for passenger-compartment materials. The nominal 20 wt% talc loading in the PP+EPDM-TD20 matrix acts as a stiffness and nucleation element, while the EPDM phase maintains multiaxial impact energy at cabin temperatures down to approximately -20 °C. The material is processed as supplied, not dry-blended with unfilled PP; regrind from sprues and runners may be incorporated up to 20 wt% only in non-visible structural ribs and bulk sections after verification of emission stability under VDA 278. Production-scale molding of dashboard carriers from this compound typically uses a two-platen injection molding machine with clamping force between 1,800 and 2,800 t, sequential valve-gated hot runners with manifold temperature held at 230–250 °C, melt temperature 210–240 °C, and mold wall temperature 20–50 °C. The gate sequence is programmed to push weld lines into defroster grille edges and away from the passenger airbag chute boundary. During filling of 2.5–3.5 mm nominal wall stock, injection pressure typically reaches 70–110 MPa, and packing pressure is set at 60–80% of filling pressure to control post-shrinkage sink marks. Batch-to-batch variation in EPDM viscosity is observable on the shop floor as a change in cushion fill time at constant injection velocity; tool transfer pressure sensors record a shift of ±5–10 MPa when regrind content or lot viscosity drifts. Terminal moldings include one-piece dashboard carriers, instrument panel retainers, defroster grille frames, and passenger-side airbag chute mounting substrates.
Because defrost duct housings, heater boxes, and footwell distribution ducts are exposed to alternating humidity and temperature from -40 °C cold-soak to 85 °C engine-adjacent heat, the governing compliance framework for European OEMs includes DIN 75201-B gravimetric fogging and VDA 278 for volatile and condensable emissions. Interior air-contact parts are also screened against VDA 277 for total carbon emissions. In this application, talc at 20 wt% reduces coefficient of linear thermal expansion sufficiently to prevent duct-to-plenum disengagement, but the filler also increases surface roughness, which can adsorb condensation promoters; stabilization selects low-volatility phenolic/phosphite packages rather than migratory lubricants. Because HVAC ducts are non-visible, molding plants commonly use up to 30 wt% of clean in-house regrind blended with virgin pellets, provided the regrind is derived from the same grade and sieved through a 4 mm screen to eliminate coarse talc agglomerates. Dual-cavity or multi-cavity injection molds use sequential valve-gated hot runners with separate temperature zones; melt temperature is held at the lower end of the processing window, 210–230 °C, to avoid degradation of the EPDM phase into low-molecular-weight condensables. Injection speed is profiled to prevent jetting in the ribbed transition between cylindrical duct walls and rectangular plenum faces; gas-assisted molding is sometimes applied to tubular sections with wall thickness transitions from 2.2 to 4.0 mm. Terminal finished parts include defrost nozzles, side-window demister ducts, heater core housings, and rear footwell air distribution adapters.
If a lower closeout panel or knee bolster substrate is molded from the same grade, visible gloss and low-temperature multiaxial impact become the binding constraints rather than bulk stiffness. Gloss uniformity is evaluated under ASTM D523 at 60°, with OEM ceilings typically below 1.5 GU for grained surfaces; scratch performance is screened under VDA 230-206, and low-temperature multiaxial impact uses ISO 6603-2 at -20 °C. The 20 wt% talc phase raises flexural stiffness but narrows the ductile-to-brittle transition, so surface-visible parts restrict uncontaminated sprue/runner regrind to 10 wt%, while internal energy-absorbing webs may use up to 15 wt% after emission and gloss stability checks. Production tooling uses acid-etched or laser-textured cavities; mold temperature is kept at 20–35 °C to reproduce grain depth, and melt temperature is controlled at 220–240 °C. Ejection force rises on shallow-draft grain surfaces, so internal mold release is incorporated in the formulation rather than sprayed externally. The packing phase is shortened relative to structural parts to prevent sink marks at rib roots after texture transfer. Terminal moldings include knee bolster covers, lower driver-side closeout panels, steering column shrouds, and under-dash trim plates.
Across center console carrier tooling, the dominant process-control variable is shrinkage anisotropy. Mold shrinkage under ISO 294-4 is different in flow and transverse directions; for talc-filled PP/EPDM at 20 wt%, flow-direction shrinkage is lower than transverse shrinkage because talc platelets orient in the filling direction, an effect visible as asymmetrical boss-to-boss dimensional drift. Heat deflection under ISO 75-2 at 0.45 MPa is the standard used to avoid deformation at cup-holder hot drink temperatures, and flammability remains governed by FMVSS 302 or ISO 3795. The formulation is processed as supplied with 20 wt% talc; no additional filler masterbatch is recommended because small changes in talc content shift both shrinkage and heat deflection outside the dimensional window. For hidden support features, up to 20 wt% regrind is accepted only if the regrind comes from center-console scrap that has not absorbed surface oil or mold release. Injection molding presses for this product class are typically 600–1,200 t; the hot runner is valve-gated at the thickest boss rather than from the side, because side gating produces a visible flow mark above the shifter gaiter line. Melt temperature is maintained at 215–235 °C, and mold temperature at 25–45 °C; screw back pressure above 5–10 bar prevents color streaking from talc agglomerates. Packing pressure and time are profiled by rib thickness: 2.8 mm main wall is packed at 50–65% of filling pressure for 3–5 s, while thick bosses are fed separately through valve gates to delay freeze-off. Terminal parts include center console carriers, cup holder housings, armrest lid substrates, and shifter bezel bases.
| Application area | Combustion standard | Emission/fogging standard | Mechanical validation standard | Dimensional/surface standard |
|---|---|---|---|---|
| Hard instrument panel carrier | FMVSS 302 / ISO 3795 | VDA 278 / VDA 277 | ISO 527-2 / ISO 6603-2 | ISO 294-4 |
| HVAC duct housing | FMVSS 302 / ISO 3795 | DIN 75201-B / VDA 278 | ISO 179-1/1eA | ISO 294-4 |
| Knee bolster / lower closeout | FMVSS 302 / ISO 3795 | VDA 278 / VDA 230-206 | ISO 6603-2 | ASTM D523 |
| Center console carrier | FMVSS 302 / ISO 3795 | VDA 278 | ISO 75-2 | ISO 294-4 |
| Airbag chute substrate | FMVSS 208 system-level | VDA 278 | ISO 6603-2 / ISO 179-1/1eA | Laser-scored residual thickness 1.0–1.5 mm |
| Glove box / closeout panel | FMVSS 302 / ISO 3795 | VDA 277 | ISO 527-2 | ISO 294-4 |
During passenger airbag chute substrate validation, the tear seam is the controlling system-level interface because the component must open under bag deployment without fragmentation at cold temperatures. The governing requirement is not a single material standard but a vehicle-level deployment test derived from FMVSS 208 occupant protection; OEM specifications commonly require deployment at cabin soak temperatures of -35 °C and +85 °C. Published data for this specific configuration is limited, so process validation must include lot-by-lot multiaxial impact screening under ISO 6603-2 and notched low-temperature Charpy testing under ISO 179-1/1eA. The nominal 20 wt% talc phase raises hinge stiffness, but reduces practical ductility compared with unfilled TPO, so regrind should not exceed 10 wt% and must be free of coarse regrind particles larger than 3 mm or oil contamination. The injection molding process positions the tear seam gate such that weld lines do not cross the hinge; sequential valve gating is used to control the melt front across the chute boundary. Melt temperature is held at 210–220 °C, below the general dashboard carrier window, to minimize EPDM chain scission. Mold temperature is set at 20–30 °C to achieve low gloss but not so low that skin freezing creates notch-sensitive weld lines. Tear seams are either molded in with a 1.0–1.5 mm residual thickness or machined post-molding by 5-axis laser scoring; laser scoring produces finer dimensional control but adds a production station. Terminal parts include passenger airbag chute substrates, hinge reinforcements, and deployment door retainers for soft-skin instrument panels.
For glove box inner racks, fuse access covers, and closeout panels, wall stock is typically thinner than structural dashboard carriers, with nominal thickness from 1.8 to 2.5 mm, so the process window moves toward lower injection pressure and faster screw recovery. Compliance for these non-visible or semi-visible parts includes FMVSS 302 or ISO 3795, and passenger-compartment emissions are assessed by VDA 277; scratch performance is less critical than for center consoles, but dimensional checks under ISO 294-4 are used for latch alignment. Because these parts are enclosed behind decorative surfaces, regrind content up to 25 wt% is commonly tolerated, provided it is not mixed with talc-filled grades of different filler loading. The production process favors multi-cavity hot-runner systems with thermal-gated tips rather than large valve gates, reducing gate blush on the non-show side. Melt temperature is set at 210–230 °C, mold temperature at 20–40 °C, and screw back pressure at 4–8 bar to maintain melt homogeneity. Filling speed is reduced near the end of fill to avoid flash in the latch openings, and recovery is completed in 1.5–2.5 s on standard reciprocating screws. Terminal finished parts include glove box inner racks, fuse access covers, instrument panel side closeouts, and passenger-side lower cover brackets.
Competitive Kingfa AIP-2015,PP+EPDM-TD20,Automotive, Interior/Dashboard prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8615365186327 or mail to sales3@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8615365186327
Email: sales3@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Kingfa AIP-2015 is an injection-moulding grade based on a polypropylene matrix modified with ethylene-propylene-diene monomer rubber and filled with 20 wt% talc. Density is typically 1.04–1.06 g/cm³ under ISO 1183-1:2019; melt mass-flow rate at 230 °C/2.16 kg is in the range 10–18 g/10 min when tested to ISO 1133-1:2022. The PP+EPDM-TD20 designation places the compound between rigid PP-TD20 and unfilled TPO grades specified for automotive interior and dashboard substrates. In dashboard applications the material is selected where grain retention, dimensional stability under solar load, and low-temperature ductility are required without the higher density and paint-adhesion complications associated with ABS/PC substrates. AIP-2015 is used primarily in hidden structural dashboard carriers, defroster grille surrounds, lower close-out panels, and passenger-side airbag door substrates. Because published lot-specific data for this commercial grade are limited, property ranges in this document are representative for PP+EPDM-TD20 compounds unless otherwise stated.
Pre-drying is recommended at 80 °C for 2–4 h when storage relative humidity exceeds 60%; melt-phase moisture above 0.05 wt% produces splay on grained dashboard surfaces and reduces weld-line strength. The melt temperature is maintained between 210 °C and 240 °C. Below 200 °C, the talc-filled matrix viscosity rises sufficiently to produce incomplete filling of thin-wall vent regions and visible flow hesitation at the end of fill. Above 250 °C, EPDM gel formation and talc–matrix interfacial degradation become measurable through an increase in melt flow rate and a decrease in notched Charpy impact after moulding. On a 75 mm twin-screw extruder with an L/D of 40:1, EPDM is typically fed downstream to limit shear heating; this prevents rubber particle size from dropping below approximately 0.5 µm, below which low-temperature impact begins to decline in PP/EPDM systems. Batch-to-batch variation in EPDM dispersion has been observed when the downstream side-feeder speed is increased beyond 40 min⁻¹; this results in surface splay on grained dashboard panels and a wider Charpy impact distribution.
On production-scale hydraulic presses with clamp force between 350 t and 1,250 t and screw diameters of 45–60 mm, injection moulding of dashboard carriers is performed with holding-pressure profiles that compensate for the higher linear shrinkage of PP+EPDM-TD20 relative to filled engineering thermoplastics. When fill time exceeds 3 s on large grained panels, surface gloss variation across the melt-flow front increases; sequential valve-gate actuation and mould temperatures of 20–50 °C reduce this effect. Observed manufacturing failures include gas splay at the end of fill from insufficient vent depth, gloss bands around gates when the screw cushion drops below 5 mm, and part ejection deformation when the demoulding surface temperature exceeds 70 °C. These process boundaries are more restrictive than those of unfilled PP but less restrictive than those of high-glass ABS/PC.
Capillary rheometry at 230 °C shows shear-thinning behavior from approximately 300 Pa·s at 100 s⁻¹ to 80 Pa·s at 1,000 s⁻¹. This permits filling of thin-wall sections down to 2.0 mm without short shots when gate velocity is controlled in dashboard carriers. In mould-filling simulation, Cross-WLF viscosity-model parameters for this class result in an optimum gate shear rate between 5,000 s⁻¹ and 50,000 s⁻¹; below this range gate freeze-off and jetting occur, and above it EPDM degradation becomes measurable. On production equipment, maximum injection pressure for a 1,200 t press is typically held below 100 MPa to reduce frozen-in stress that contributes to dashboard rattle after thermal cycling.
Thermal expansion of the filled compound is anisotropic due to talc orientation. In the flow direction, CLTE measured by ISO 11359-2:1999 between -30 °C and 80 °C is often 50–65 µm/m·K; transverse to flow it rises to 80–100 µm/m·K. This anisotropy produces warpage in large dashboard carriers if the gate layout does not balance flow orientation. Mould-filling analysis should use these directional values rather than a single isotropic CLTE. Post-moulding shrinkage of 0.8–1.2% over 24 h and subsequent annealing at 80 °C for 2 h stabilize dimensions for downstream foam-in-place bonding.
In multi-gate injection of dashboard carriers, weld lines are created at the intersection of melt fronts behind defroster vents and passenger airbag apertures. In PP+EPDM-TD20, weld-line strength retention depends on talc orientation and EPDM migration. At a melt temperature of 230 °C and mould temperature of 40 °C, weld-line tensile strength is typically 55–70% of the bulk value when tested to ISO 527-2:2012. Lower mould temperatures reduce this to 40–55% because talc platelets align perpendicular to the weld plane before the fronts coalesce. Increasing EPDM content above 20 wt% improves ductile response but may raise surface tack and odour. In AIP-2015, the talc level is held at 20 wt% to avoid the severe weld-line loss associated with 30–40 wt% talc compounds used in under-hood parts.
At low temperature, impact performance is influenced less by EPDM content than by dispersion quality in the polypropylene matrix. The addition of EPDM improves Charpy notched impact at -30 °C from approximately 3–5 kJ/m² for PP-TD20 to 6–9 kJ/m² for PP+EPDM-TD20 when tested to ISO 179-1:2010. Dynamic mechanical analysis typically shows a beta-transition in the region -50 °C to -35 °C associated with the EPDM phase; the PP matrix retains its main glass transition near 0 °C unless a high-ethylene EPDM grade is used. The brittle-to-ductile impact transition occurs near -20 °C for PP+EPDM-TD20, whereas PP-TD20 remains brittle at 0 °C. This difference is the principal reason for specifying AIP-2015 in passenger-side airbag doors and dashboard lower carriers exposed to cold-soak conditions.
The stabilizer package in interior-grade PP+EPDM-TD20 formulations is selected to limit oxidative embrittlement underneath instrument panel top surfaces where solar load produces continuous skin temperatures near 110 °C. Long-term heat ageing at 120 °C for 500 h generally produces a decline in tensile elongation at break of less than 25% when tested to ISO 527-2:2012. For darker colours, surface temperature above 110 °C may cause gloss increase and visible talc whitening on high-grain areas. Published data for this specific commercial configuration is limited; therefore, the values should be read as representative for the PP+EPDM-TD20 class rather than lot-specific certification data.
PP-TD20 without EPDM offers higher flexural modulus and lower raw-material cost but suffers from brittle failure below 0 °C and lower weld-line ductility. Unfilled PP offers lower density and better flow but cannot meet dashboard dimensional stability requirements; its CLTE typically exceeds 100 µm/m·K measured by ISO 11359-2:1999, whereas PP+EPDM-TD20 is commonly in the range 70–90 µm/m·K. ABS/PC substrates provide higher HDT and paint adhesion but increase part mass by approximately 8–12% and often require mould temperatures above 70 °C, increasing energy input and cycle time. AIP-2015 is specified where low-temperature airbag deployment, low-cost grained surfaces, and recyclability through the polypropylene stream are more important than the high-modulus stiffness of ABS/PC.
| Material class | Flexural modulus | Notched Charpy at -30 °C | Typical CLTE | Main limitation |
|---|---|---|---|---|
| PP-TD20 | 2000–2200 MPa | 3–5 kJ/m² | 60–70 µm/m·K | Low-temperature brittleness |
| PP+EPDM-TD20 | 1600–1900 MPa | 6–9 kJ/m² | 70–90 µm/m·K | Lower modulus than PP-TD20 |
| Unfilled PP | 1100–1300 MPa | 2–4 kJ/m² | 100–120 µm/m·K | Dimensional stability |
| ABS/PC | 2200–2500 MPa | 15–25 kJ/m² | 65–80 µm/m·K | Higher density and paint requirements |
Test methods are ISO 178:2019 for flexural modulus, ISO 179-1:2010 for notched Charpy impact, and ISO 11359-2:1999 for CLTE. Values are representative ranges for the product class, not lot-specific certification data.
Because the dashboard substrate is heated by solar load, volatile organic compound and fogging behavior are critical. Low-VOC stabilizer packages and high-purity EPDM grades are used in AIP-2015. Gravimetric fogging tested to DIN 75201:2011-06 typically yields condensate values below 2 mg, while VDA 278:2011-08 total volatile organic compound values for PP+EPDM-TD20 dashboard grades are commonly below 100 µg/g. These values are not lot certificates and should be verified on production-sampled material. Formulations containing reclaimed EPDM or broad molecular weight distribution polypropylene can increase fogging and odour above the vehicle interior acceptance limit; therefore, AIP-2015 is run with dedicated interior-grade raw-material streams.
| Requirement | Standard / regulation | Typical interior threshold or method |
|---|---|---|
| Heavy metals | RoHS Directive 2011/65/EU Annex II | Pb ≤ 1000 ppm, Cd ≤ 100 ppm |
| ELV heavy metals | 2000/53/EC Annex II | Pb ≤ 0.1 wt%, Cd ≤ 0.01 wt% |
| REACH SVHC | Regulation (EC) No 1907/2006 Article 33 | No SVHC > 0.1 wt% in intended formulation |
| Fogging | DIN 75201:2011-06 | Condensate < 2 mg |
| Occupant compartment odour | VDA 270:2016 | Odour grade ≤ 3.0 |
In soft-touch dashboard lamination, the substrate must maintain acceptable peel adhesion to polyurethane foam and decorative skin layers after ageing. AIP-2015 substrates are tested for foam-to-substrate adhesion after 7 d at 80 °C and 95% relative humidity; adhesion loss occurs if talc migration to the surface creates a weak boundary layer. Plasma or corona pre-treatment is not normally required for foamed-in-place polyurethane, but adhesion promoters may be specified when a decorative skin is bonded with solventborne polyurethane adhesives. Because PP+EPDM-TD20 is nonpolar, solvent wipe cleaning before adhesive application should use isopropanol rather than aromatic hydrocarbons to avoid surface etching and visual defects on grained surfaces.