| HS Code | 778985 |
| Product | Kingfa API-2125 |
| Base Polymer | PP+EPDM-TD |
| Filler | Talc |
| Filler Content | 20% |
| Density | 1.04 g/cm3 |
| Melt Flow Rate | 12 g/10 min (230°C/2.16 kg) |
| Tensile Strength | 22 MPa |
| Elongation At Break | 100% |
| Flexural Modulus | 1800 MPa |
| Notched Izod Impact Strength | 30 kJ/m2 (23°C) |
| Heat Deflection Temperature | 110°C (0.45 MPa) |
| Vicat Softening Temperature | 130°C |
| Molding Shrinkage | 1.0-1.4% |
| Flammability | HB |
As an accredited Kingfa API-2125,PP+EPDM-TD,Automotive, Interior factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 25 kg moisture-resistant paper bags, palletized and stretch-wrapped for safe transport of automotive interior-grade PP+EPDM-TD compound. |
| Container Loading (20′ FCL) | Kingfa API-2125 PP+EPDM-TD automotive interior compound loaded in a 20′ FCL with standard export packing for secure shipment. |
| Shipping | Kingfa API-2125 (PP+EPDM-TD automotive interior compound) is supplied as pellets in sealed moisture-barrier bags or octabins. Ship as non-hazardous thermoplastic in dry, covered freight; avoid heat, sunlight, moisture, and contamination. No special dangerous-goods classification applies. |
| Storage | Store Kingfa API-2125 in a clean, dry, well-ventilated warehouse at ambient temperature, protected from direct sunlight, heat, ignition sources, moisture, and incompatible chemicals. Keep original packaging sealed, intact, and on pallets; avoid heavy stacking and follow FIFO. Protect from rain, contamination, and static buildup. Store separately from acids, alkalis, oxidizers, and solvents. Use suitable PPE and avoid dust generation during handling. |
| Shelf Life | Typically 24 months in original sealed packaging, stored dry below 30°C, protected from sunlight and moisture. |
Lower instrument panel substrate molding with 15–25 wt% talc-filled PP/EPDM compounds in the API-2125 class requires gate-to-flow length ratios below 120:1 when wall thickness is 2.4 mm, otherwise short-shot and gloss instability develop on the driver-side knee bolster area. The compliance envelope for this exposure zone is anchored by ISO 3795 / FMVSS 302 for horizontal burn rate, DIN 75201-B for fogging condensate, and VDA 278 thermal desorption for VOC/FOG emissions. OEM interior specifications commonly set fogging values not exceeding 2.0 mg per DIN 75201-B and VDA 270 odor intensity at or below 3.0; VDA 278 acceptance windows for PP-based interior compounds are often stated as ≤100 µg/g VOC and ≤250 µg/g FOG, though the exact API-2125 lot certificate should be consulted because published data for this specific configuration is limited. On the shop floor, API-2125 is metered as the 100% compound; where in-line molding trials permit, a maximum 20 wt% of clean, same-lot regrind is introduced but only after checking each regrind batch for a melt mass-flow rate within ±5% of virgin material and no visible black specks. The typical injection molding line uses a 1600–1800 t clamp force machine with a screw L/D of 20:1–24:1, melt temperature 210–230°C, mold temperature 20–35°C, injection speed profiled from 150 mm/s to 80 mm/s at switchover, and a three-stage holding pressure profile of 55 MPa, 45 MPa, and 30 MPa to compensate for the knee bolster hinge boss sink. Production-scale trials have shown that when hot runner valve pin timing is delayed beyond 0.8 s after switchover, cold slug formation at the center gate can produce visible splay in the knee bolster radius; this is mitigated by staging holding pressure rather than using a single hold. Pre-drying at 80°C for 2–4 h is recommended when ambient relative humidity exceeds 60% or when pellet surface moisture is above 0.05 wt%, because talc-filled polypropylene can carry residual moisture into the melt and generate splay at the knee bolster gate. The terminal finished part family includes lower knee bolster carriers, driver-side under-column covers, lower glove box retainers, and hidden side supports for the instrument panel substrate.
Door lower and map pocket components molded from PP/EPDM-talc exhibit a property cliff at talc loadings above 25 wt%: scratch visibility increases because talc platelets align perpendicular to flow near the textured surface and raise local gloss after mechanical damage. OEM scratch resistance is evaluated under GMW 14688 five-finger scratch at 10 N; a delta L below 1.5 is typically required for Class A grain depths of 40–60 µm. Flammability is established through ISO 3795, fogging through DIN 75201-B, and odor through VDA 270. Formulation control for door lowers usually maintains API-2125 as the sole matrix; where a color masterbatch is added, it is limited to 2–3 wt% and must be pre-dried separately at 80°C for 2 h. Regrind content is capped at 20 wt% because two-pass thermal history lowers impact resistance at -30°C by 8–12% in Charpy notched tests compared to virgin compound. For deep map pockets, a direct cold sprue gate into the non-visible backside is preferred; the melt is injected at 210–230°C with a fill time of 1.8–2.6 s. Deep-draw sections with depth-to-width ratio above 0.75 require a clamp force of at least 3.0 kN/cm² of projected area to prevent flash at ejector pin locations. Texture is applied as a chemical-etched cavity finish with a nominal draft angle of 5° on grain walls, and demolding is assisted by large-diameter ejector sleeves around clip bosses. On a production line, a 1000–1300 t hydraulic press may be sufficient for a two-cavity door lower mold, but hot runner balancing is necessary; an unbalanced fill of more than 3% between cavities causes sample-to-sample grain gloss difference of 0.8–1.2 GU on the map pocket outer face. Terminal finished goods include door lower trim panels, map pocket shells, rear door lower inserts, and speaker grille substrates where local OEM specifications permit the compound’s stiffness and grain retention.
| Application zone | Flammability | Emissions / fogging / odor | Mechanical / scratch / chemical | Substance / recycling |
|---|---|---|---|---|
| Lower instrument panel substrate | ISO 3795, FMVSS 302 | DIN 75201-B, VDA 278, VDA 270 | ISO 527-2/1A/50, ISO 179-1/1eA | REACH SVHC ≤0.1 wt% |
| Door lower and map pocket | ISO 3795 | DIN 75201-B, VDA 270 | GMW 14688, ISO 179-1/1eA | ≤20 wt% same-lot regrind |
| Lower pillar trim | ISO 3795 | VDA 278, VDA 270 | ISO 179-1/1eA | ≤15 wt% same-lot regrind |
| Center console side cover | ISO 3795 | VDA 278, VDA 270 | GMW 14688, ISO 2812-1, DIN 53160 | ≤15 wt% regrind |
| Seat side shield | ISO 3795 | VDA 278, VDA 270 | ISO 527-2/1A/50, ISO 179-1/1eA | ≤15 wt% regrind |
| Cargo / trunk interior trim | ISO 3795 | DIN 75201-B, VDA 278 | ISO 6603-2 | ≤20 wt% same-lot regrind |
In lower pillar trim, post-molding dimensional stability is governed by the coefficient of linear thermal expansion, which for PP/EPDM-talc is typically 60–80 µm/m·K in the transverse direction, about half that of unfilled PP. Low-temperature impact performance for airbag deployment path clearance is assessed using ISO 179-1/1eA notched Charpy at -30°C, with typical acceptance threshold of ≥4.0 kJ/m²; flammability is tested to ISO 3795; emissions and odor under VDA 278 and VDA 270. The compound is processed as a 100% compound with 15% same-lot regrind allowed; color masterbatch is held at 1.5–2.5 wt% to avoid gloss drift on grain peaks. Injection molding of pillar lower covers uses wall thickness 2.0–2.5 mm, melt temperature 210–230°C, mold temperature 25–35°C, packing between 50–60 MPa, and holding time 8–12 s. Clip tower sections require sacrifice ribs at 0.8 mm thickness to prevent sink marks without increasing cycle time. Sequential valve gating may be employed on A-pillar lower covers longer than 600 mm. Post-molding shrinkage measured after 48 h at 90°C should not exceed 0.4% in the longitudinal axis; exceeding this value indicates excessive free shrinkage and can lead to airbag deployment path interference at the lower B-pillar. Mold temperature variation of more than 5°C across the cavity is a known source of differential shrinkage. Production lines with electric injection units report less screw recovery variability, and clip tower cracking has been traced to insufficient melt cushion below 4 mm. Finished types include A-pillar lower covers, B-pillar lower post covers, C-pillar lower covers, and seat belt adjuster covers.
Center console side cover molding with a scratched talc-filled PP/EPDM surface places simultaneous demands on low-gloss retention, chemical resistance to skin oil and hand sanitizer, and structural stiffness at the rear armrest hinge boss. Chemical resistance is screened in a modified ISO 2812-1 contact test using artificial sweat according to DIN 53160, with visual grazing assessed after 24 h at 23°C; scratch resistance remains evaluated under GMW 14688 at 10 N. Flammability compliance is established through ISO 3795, and interior air quality through VDA 278 and VDA 270. For a two-shot center console side panel, API-2125 forms the rigid substrate at nominal wall thickness 1.8–2.0 mm, while a TPV soft-touch layer is overmolded at 0.8–1.2 mm; the thickness ratio is approximately 75:25 rigid substrate to soft skin. If a single-shot side cover is specified, API-2125 is used at 100%, with 2–3 wt% black or accent color masterbatch and ≤15 wt% regrind. Rotary platens with 2+2 cavity layout are used for two-shot production; for single-shot tools, the gate is placed on the non-visible underside, fill time is 1.5–2.2 s, mold temperature is 30–40°C, and draft angle on the grained side wall is held at 5° minimum to prevent scuffing during ejection. Chemical degradation from hand sanitizer can be accelerated by talc-rich surface layers; a contact time of 1 min with ethanol/isopropanol 70% solution followed by 24 h recovery is part of OEM chemical resistance screening. If haze appears at 1.5 mm thickness, the part is rejected. Terminal finished part types include center console side covers, rear console side covers, armrest carrier shells, and lower storage bin outer shells.
Seat side shields molded from talc-filled PP/EPDM compounds are less prone to gross cracking than unfilled PP but remain sensitive to ejection-induced stress whitening at clip towers and screw bosses when demolding force exceeds the yield stress of the rapidly cooled skin. Mechanical acceptance typically references ISO 527-2/1A/50 tensile yield at 23°C and ISO 179-1/1eA notched Charpy at -30°C; flammability is tested to ISO 3795, emissions to VDA 278, and odor to VDA 270. The compound is fed at 100%; clean in-house regrind is capped at 15 wt% and monitored for melt mass-flow rate drift, while color masterbatch loading of 2 wt% is typical. The tool should place gates at the non-visible rear edge or underside; fill time is 1.5–2.0 s, packing pressure 40–70 MPa, and mold temperature 20–40°C. For handle bezels with integrated clips, large flat ejectors and drafted side walls of 3° minimum are required to reduce scuffing and stress whitening. Ejector speed above 80 mm/s worsens white marks; ejection velocity is limited to 50–70 mm/s on textured seat side shields. Mold release spray is not used because it causes gloss variation on grain. Terminal finished types include seat side shields, height-adjustment handle bezels, recline handle covers, and seat belt lower anchor covers.
For carpeted trunk side trim carriers produced at flow lengths of 900–1100 mm and wall thickness 2.5 mm, the limiting parameter is not melt flow but post-molding shrinkage anisotropy between flow and transverse directions, which for talc-filled PP can differ by 0.3–0.5 percentage points. Low-temperature impact for luggage retention is evaluated under ISO 6603-2 multiaxial impact at -30°C; flammability per ISO 3795; fogging per DIN 75201-B; emissions per VDA 278. API-2125 is used at 100%; same-lot regrind may be added up to 20 wt% if the mixture density is within ±0.01 g/cm³ of virgin and carbon black masterbatch at 2–3 wt% is incorporated for color consistency. Sequential valve-gated injection molding at melt temperature 210–230°C and mold temperature 25–35°C uses a holding profile of 60–35 MPa; cooling time is calculated from part thickness squared with PP thermal diffusivity of approximately 0.08 mm²/s. Sequential valve-gated tools with gate delay of 0.5–1.0 s between nozzles reduce flow-front hesitation at the trunk floor interface. Terminal finished types include trunk side trim, spare-wheel covers, tailgate inner covers, and cargo floor supports.
Competitive Kingfa API-2125,PP+EPDM-TD,Automotive, Interior prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8615365186327 or mail to sales3@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8615365186327
Email: sales3@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Kingfa API-2125 is a compounded polypropylene/ethylene-propylene-diene monomer/talc grade intended for injection-moulded automotive interior components. The designation PP+EPDM-TD indicates a polypropylene matrix, an EPDM impact-modifier phase, and a controlled talc mineral filler fraction; the grade is supplied as pelletised feedstock, not as a dry blend or masterbatch. This compositional structure is selected for interior trim applications in which the part must survive low-temperature impact, intermediate heat exposure from solar load, and dimensional stability requirements across wide cabin temperature swings. Typical application candidates include pillar trim, door panel inserts, seat side shields, console side panels, and other semi-structural interior trim. Published supplier data for this specific grade are limited; the numerical ranges presented in this document are class-typical values for PP+EPDM-TD automotive interior compounds and must be verified against a current certificate of analysis for a given production lot.
The compound is formulated around a talc loading commonly maintained between 10 wt% and 25 wt%, with EPDM content in the range of 15 wt% to 30 wt%. Talc contributes stiffness, reduced shrinkage, and a matte surface; the EPDM phase restores low-temperature impact and knit-line toughness but reduces melt flow and tensile yield. The following table summarises the property envelope typical of this material class under laboratory conditioning at 23 °C and 50% relative humidity unless otherwise indicated.
| Property | Test standard | Unit | Typical envelope |
|---|---|---|---|
| Density | ISO 1183-1:2019 | g/cm³ | 1.04–1.12 |
| Melt flow rate, 230 °C/2.16 kg | ISO 1133-1:2022 | g/10 min | 10–20 |
| Tensile stress at yield | ISO 527-2:2012 | MPa | 18–25 |
| Flexural modulus | ISO 178:2019 | MPa | 1800–2600 |
| Charpy notched impact strength, 23 °C | ISO 179-1:2010 | kJ/m² | 5–15 |
| Heat deflection temperature, 0.45 MPa | ISO 75-2:2013 | °C | 95–115 |
| Mould shrinkage, 60×60×2 mm plaque | ISO 294-4:2018 | % | 0.8–1.3 |
These values are not a certificate of analysis and are influenced by pigment loading, tensile bar gating, and tool conditions. Lot-to-lot variation in talc aspect ratio and EPDM molecular weight may shift flexural modulus and Charpy impact by more than 10%.
The polypropylene matrix is typically an impact copolymer or a controlled-rheology homopolymer blended with EPDM. Talc surface treatment may include silane or stearate coupling agents to improve filler wetting and reduce moisture pickup. EPDM dispersion quality is assessed by reflected-light microscopy or scanning electron microscopy on microtomed plaques; a mean dispersed elastomer domain size below 2 μm is generally associated with stable impact performance in mineral-filled systems, although API-2125-specific domain-size data are not published. The combination of talc and EPDM is not a crosslinked vulcanizate; the EPDM remains a dispersed thermoplastic-compatible elastomer phase, which distinguishes this class from TPVs.
On the injection-moulding line, the compound is processed with a melt temperature profile of 200 °C to 230 °C and a mould wall temperature of 30 °C to 50 °C. When opened containers are stored at relative humidity above 60%, pre-drying in a desiccant dryer at 80 °C for 2–4 h is recommended because the talc fraction can retain surface moisture and generate splay on grained surfaces. Hot-runner manifold temperatures should not exceed 230 °C for extended idle periods; residence times above 8 min at high barrel temperatures have been associated with gloss variation and EPDM phase degradation in similar talc-filled PP compounds. Screw recovery and back pressure should be controlled to avoid melt temperatures above 250 °C, at which point volatile evolution from the modifier and stabiliser package may increase. Clamp force selection follows standard PP-talc practice; for medium-sized interior panels, machines in the 800–1,500 kN range are commonly employed, but the required force is determined by projected area and flow length rather than material class alone.
In twin-screw compounding, talc is introduced through side stuffing to limit barrel abrasion and to avoid excessive screw wear; EPDM is metered either as pellets or as a pre-dispersed masterbatch. Production-scale compounding typically employs co-rotating twin-screw extruders with L/D ratios of 40:1 to 56:1, vacuum devolatilisation, and strand pelletising. Talc content is verified by loss on ignition or TGA, with ash values checked against the target formulation. Batch-to-batch variance in this compound family is driven mainly by talc particle size distribution and EPDM molecular weight; if these inputs drift, the injection moulder observes changes in melt viscosity, screw recovery time, and part weight stability.
Compared with unfilled PP impact copolymer, the talc platelets in API-2125 reduce linear mould shrinkage and make the shrinkage anisotropy less severe. Class-typical ISO 294-4 mould shrinkage values for unfilled PP impact copolymer can lie between 1.2% and 1.7%, while a talc-filled EPDM compound is usually specified at 0.8% to 1.3%. The coefficient of linear thermal expansion is correspondingly lowered; a talc-reinforced PP grade may exhibit 50–70×10⁻⁶ K⁻¹ in the flow direction versus 100–150×10⁻⁶ K⁻¹ for unfilled polypropylene, when tested under ISO 11359-2. This reduction improves dimensional stability in large interior panels exposed to cabin heating. However, talc platelets orient during fountain-flow filling and can produce differential shrinkage between flow and cross-flow directions, leading to warp in thin-walled parts with asymmetric gate locations. Weld-line strength is also affected: talc concentrates along the weld plane, reducing the available polymer-to-polymer fusion area; the EPDM phase partially compensates by blunting crack initiation. The net result is that weld-line Charpy impact in API-2125 is lower than in an unfilled EPDM-modified PP but higher than in a mineral-filled PP homopolymer without impact modifier.
Weld-line strength in talc-filled systems is also influenced by melt temperature: below 200 °C, the frozen skin at the flow front can inhibit re-welding and increase the visibility and weakness of weld lines on grained surfaces. Increasing melt temperature to 220–230 °C improves weld-line healing but may intensify odour and volatile emission if the EPDM or stabiliser package is heat-sensitive. This trade-off is managed through process capability studies on production tools with pressure transducers located near the gate and at the end of flow; a drop in end-of-fill pressure below 30 MPa on large panels is often associated with increased weld-line stress and higher reject rates for sink marks and warpage.
Automotive interior parts in parked vehicles can see air temperatures above 90 °C and surface temperatures near 110 °C on dark trim. Under these conditions, the polypropylene matrix undergoes oxidative degradation, and the EPDM phase can lose ductility through crosslinking and chain scission. Class-typical PP+EPDM-TD compounds are evaluated for heat ageing at 100 °C or 120 °C in forced-air ovens per ISO 188 or ASTM D3045, with retention of tensile elongation and notched impact as primary indicators. Published data for API-2125-specific ageing performance are limited; the grade should be qualified by the end user on production parts using the expected thickness and surface pigmentation. Continuous use above 100 °C is generally outside the reliable design envelope for this polymer class unless the part is unstressed and short intermittent exposure is accepted. Long-term heat exposure also tends to increase talc-filled PP surface haze and reduce impact at weld lines more rapidly than in unfilled PP because of the higher surface area of the mineral phase and stabiliser depletion at the interface.
Dimensional changes during heat ageing are also relevant. Differential scanning calorimetry of talc-filled PP often shows secondary crystallisation at temperatures above 90 °C, which can increase shrinkage and embrittlement over time. By contrast, annealing protocols per ISO 188 may be used to stabilise crystallinity before dimensional inspection. For parts with tight gap and flushness requirements, a post-mould thermal ageing step at 80–100 °C for 1–2 h is sometimes used, but this practice can alter surface gloss and must be validated for each grained texture.
Against an ABS/PC blend commonly used for interior trim, API-2125 offers lower density, generally in the range of 1.04–1.12 g/cm³ versus 1.08–1.15 g/cm³ for a mineral-filled ABS/PC, and better resistance to long-term stress cracking in contact with many automotive cleaning agents. However, its heat distortion temperature under 0.45 MPa is lower by roughly 10–20 K than a typical ABS/PC grade, and its surface pencil hardness is lower. Conversely, the low-gloss talc surface helps mask marring and fingerprinting in cabin touch areas. Compared with standard PP-talc compounds without EPDM, API-2125 is differentiated by improved low-temperature impact. A conventional PP+20 wt% talc homopolymer can exhibit a ductile-to-brittle transition near 0 °C; the EPDM-modified grade is formulated to push that transition below -20 °C, although exact values depend on talc content and EPDM dispersion quality. This shift is critical for door pockets and side pillars that may be struck during cold-weather loading.
In applications requiring a soft-touch surface, API-2125 should not be confused with thermoplastic vulcanizate or sheet-based soft-touch laminates. The EPDM content in the PP+EPDM-TD compound is not sufficient to produce low Shore hardness; the talc and polypropylene matrix keep the flexural modulus above 1800 MPa. Therefore, noise-damping soft-touch components such as upper instrument panel skins or armrest covers typically use TPV or TPU skins, while API-2125 is better suited to rigid substrates and structural trim carriers beneath the soft layer. This distinction is relevant on multi-component instrument panels where the substrate must provide dimensional stability and the skin must provide tactile properties.
Interior trim compounds are screened for volatile and semi-volatile organic emissions because cabin air quality limits are specified by vehicle manufacturers. PP+EPDM-TD grades in this class are typically evaluated by VDA 277 for total volatile organic compounds, DIN 75201-B for gravimetric fogging, and VDA 278 for VOC and FOG fractions by thermal desorption gas chromatography. The EPDM phase can contribute residual aliphatic hydrocarbons and additives; therefore low-emission stabiliser packages and high-purity process oils are required. Published data for API-2125-specific emission performance are limited, and final validation must be performed on injection-moulded parts after any graining, painting, or laminating operation because texture depth and part conditioning can change emission values by more than 20%. Odour assessments are commonly conducted under VDA 270 using storage at 80 °C for 2–24 h; for talc-filled PP, the mineral filler itself is not the main odour source, but it can adsorb processing by-products and release them slowly during cabin heat exposure. Formaldehyde emissions from PP are generally low, but additives and masterbatch carriers may contribute trace levels detectable by VDA 275.
Because talc has a high specific surface area, it can adsorb organic compounds during compounding and release them slowly under cabin temperatures. The characteristic emission profile of PP+EPDM-TD therefore may show aliphatic hydrocarbons from the EPDM phase, antioxidant degradation products, and low levels of fatty acid derivatives from surface-treated talc. Gas chromatography–mass spectrometry library matching under VDA 278 is used to identify specific compounds rather than total VOC alone. Manufacturers may impose internal limits for naphthalene, toluene, ethylbenzene, and xylene concentrations in the raw material; however, published data for API-2125 are limited, and these limits vary by OEM specification.
The base grade does not carry a weatherable ASA or acrylic cap layer; accelerated weathering per ISO 4892-2 or SAE J2527 on unpigmented PP+EPDM-TD can produce surface chalking, gloss reduction, and impact loss with cumulative UV dose. Therefore, the material is not intended for exterior Class A surfaces or for interior parts receiving sustained direct sunlight through untinted glazing without additional stabilisation or surface coating. The compound is also incompatible with amine-based additives and some hindered amine stabiliser systems if used at high levels because they can interfere with acid scavenger performance and shift talc dispersion stability; formulation changes should be evaluated on production-scale equipment rather than small laboratory mixers.