| HS Code | 268562 |
| Grade | Kingfa API-2515 |
| Composition | PP + EPDM + 20% Talc |
| Density | 1.05 g/cm³ |
| Melt Flow Rate 230 C 2 16 Kg | 15 g/10 min |
| Tensile Strength At Yield | 20 MPa |
| Tensile Elongation At Break | 50% |
| Flexural Modulus | 1800 MPa |
| Notched Izod Impact Strength At 23 C | 30 kJ/m² |
| Notched Izod Impact Strength At 30 C | 8 kJ/m² |
| Heat Deflection Temperature At 0 45 Mpa | 110 °C |
| Vicat Softening Temperature | 145 °C |
| Molding Shrinkage | 1.0–1.3% |
| Uv Stabilization | Yes |
As an accredited Kingfa API-2515,PP+EPDM-TD20 (Rigid-Tough Balance, UV),Automotive factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaging: 25 kg moisture-resistant bags, 40 bags per pallet (1,000 kg net), for Kingfa API-2515 PP+EPDM-TD20 automotive compound. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): 25 kg bags of Kingfa API-2515 PP+EPDM-TD20 automotive compound, palletized and shrink-wrapped, up to 20–22 tons. |
| Shipping | Kingfa API-2515 PP+EPDM-TD20 automotive compound is shipped as dry, free-flowing pellets in sealed moisture-barrier bags or lined octabins, palletized and stretch-wrapped. It is non-hazardous under normal transport; protect from moisture, UV, and contamination. Store cool and dry, away from direct sunlight, per SDS and local regulations. |
| Storage | Store Kingfa API-2515 (PP+EPDM-TD20) in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat sources, moisture, and contaminants. Keep pellets in original sealed packaging on pallets; avoid sharp objects and excessive stacking. Protect from prolonged UV exposure and mechanical damage. Maintain moderate temperature/humidity, use FIFO, and follow local fire and handling regulations. |
| Shelf Life | Shelf life is typically 12 months when stored dry, cool, and ventilated in original unopened packaging, protected from sunlight. |
In painted front and rear bumper fascia production, Kingfa API-2515 is processed as-delivered at 100 wt% on hydraulic injection molding machines with clamp forces between 2,000 t and 3,500 t. The compound is pre-dried in a desiccant dryer at 80°C for 2 h when ambient relative humidity exceeds 60%; barrel temperature set-points are 200°C, 215°C, 225°C, and 230°C from feed to nozzle, with a screw L/D of 20:1 and compression ratio of 2.5:1 to limit shear heating of the EPDM phase. The mold is held at 20–35°C for smooth Class A surfaces because higher mold temperatures increase talc exposure and reduce paint adhesion. Compliance verification uses ISO 527-1:2019 for tensile properties, ISO 178:2019 for flexural modulus, ISO 179-1/1eA for notched Charpy impact at 23°C and -30°C, and ISO 6603-2 for instrumented multiaxial puncture at -30°C using a 20 mm hemispherical striker. Outdoor weatherability is screened through SAE J2527:2017 xenon-arc exposure at 2,500 kJ/m² with ISO 105-A02:1993 gray-scale rating of 4 or higher; paint adhesion is qualified to ISO 2409:2020 cross-cut class 0 or 1. Prior to painting, the substrate is activated by flame ionization at 8–12 kW burner output with a 12–20 mm oxidizing flame at line speeds of 10–15 m/min, followed by a chlorinated polyolefin adhesion promoter applied at 2–3 µm dry film thickness. One-component basecoat and two-component clearcoat are then applied. Internal mold release agents or silicone-based slip additives are not permitted because residues contaminate the low-surface-energy PP substrate even after flame treatment. Regrind use is restricted to 15 wt% of post-production unpainted scrap unless UV re-stabilization evaluation is repeated. Terminal finished parts include front and rear painted bumper fascias and lower grille opening panels, with continuous service bounded at -40°C to 85°C.
Grained rocker panel and body side cladding testing identifies the limiting condition as low-temperature impact retention at the knit line, not bulk material ductility. The compound is normally dosed as 100 wt% direct feed; an external color concentrate is allowable up to 2 wt% only if the carrier resin is a low-melt PP homopolymer. Higher addition lowers EPDM phase continuity and reduces notched Charpy impact at -30°C to ISO 179-1/1eA. The part must meet cold-impact requirements after 500 h of SAE J2527:2017 xenon-arc exposure, and surface cracking is graded to ISO 4628-4:2016. Production tooling uses edge-gated or fan-gated injection with a valve-gated hot runner to position gas venting along the weld line. The mold temperature is set at 35–50°C to reproduce low-gloss grain depth of 15–25 µm, but it must not exceed 60°C because talc platelets orient to the surface and produce silvery flow marks. Screw wear from talc is controlled by using bimetallic barrels and screws with surface hardness above HRC 62. Coefficient of linear thermal expansion measured to ISO 11359-2:2021 remains low enough for body-side clip attachment over a -40°C to 85°C range. The known handling boundary is that weld lines must be moved to low-stress, non-cosmetic regions; if a weld line appears on the exposed rocker lower face, injection velocity above 150 mm/s or gate relocation is required. Finished products include lower rocker panel cladding, door lower garnish, and side sill extensions. Published data for this specific grade at that weld-line location are limited.
Cowl vent grille and plenum chamber water deflector tooling in forward-cabin air intake regions is generally assigned to high-flow PP/EPDM-TD20 compounds because the drainage grid combines 2.0–2.5 mm nominal wall thickness with snap-fit retention tabs and large flat areas subject to solar load. The material is used at 100 wt% without further letdown; if post-industrial PP recyclate is added for cost reduction, the maximum is 10 wt% because dilution reduces UV stabilizer concentration below the requirement for 1,500 kJ/m² xenon-arc exposure to SAE J2527:2017 with ISO 105-A02:1993 gray-scale rating of 3–4 minimum. Melt temperature is set between 215°C and 230°C, injection speed at 100–130 mm/s, and mold temperature at 25–40°C for flatness control. The tool requires venting depth of 0.02–0.03 mm along the drainage ribs to prevent gas burn at rib tips. Dimensional stability is verified by ISO 527-1:2019 tensile creep testing and ISO 11359-2:2021 thermal expansion evaluation. Terminal products include cowl vent grilles, plenum covers, and water deflector assemblies. Continuous underhood soak temperatures above 95°C are not recommended because the talc-filled PP matrix may creep at attachment points and produce buzz/squeak/rattle failures during cabin evaluation.
A low-gloss black front grille surround imposes two simultaneous constraints: gloss uniformity across a grained surface and resistance to UV-driven chalking after repeated car-wash cycles. The formulation is run at 100 wt% of the UV-stabilized compound; an external low-gloss color concentrate may be used at 1–2 wt% if its carrier melt flow rate does not deviate more than 5 g/10 min from the base resin when tested to ISO 1133-1:2022 at 230°C/2.16 kg. The injection molding machine should provide 35–45 MPa cavity pressure and a screw L/D of 20:1 with a non-reciprocating check ring to prevent talc segregation. The mold is run with a stepped temperature profile: 20°C in the high-gloss surround ring and 55–60°C in the grained grille mesh to reproduce texture depth without flow lines. UV resistance is validated by SAE J2527:2017 at 3,000 kJ/m² and ISO 105-A02:1993 rating of 4 or higher; post-exposure tensile elongation retention is checked to ISO 527-1:2019. The terminal parts include black front grille surrounds, lower bumper grille inserts, and headlamp washer cover plates. Design constraints include minimum rib thickness of 1.0 mm and gate diameter of 1.5 mm to avoid jetting, because talc-filled melts do not re-mix after jetting. Gloss is monitored across the mesh to ISO 2813:2014 at 60° measurement angle; variation above 0.8 GU within the same part is considered a visual defect.
Wheel arch liners and rear spats are consolidated into direct-injection assemblies where the main failure modes are stone impact at highway speed and deformation after prolonged exposure to brake and road heat. The compound is processed at 100 wt% direct; if overmolding is used, the core can be PP-GF20 at 30 wt% of the total shot mass. Compliance includes ISO 6603-2 multiaxial impact at -30°C, ISO 178:2019 flexural modulus, and ISO 11359-2:2021 CLTE for clip retention. The tool is a two-plate cold-runner mold with melt temperature 220°C and mold temperature 25°C; cycle time for 2.5 mm wall is 35–45 s. Terminals include front wheel arch liners, rear spats, and mud guard extensions. A known limitation is that continuous contact with tire dressing solvents can soften the EPDM surface, so solvent exposure is tested by ISO 175:2020 before color approval.
Under two-component injection molding conditions for a rear bumper step pad, the outer layer is processed at 100 wt% of the rigid-tough PP/EPDM-TD20 compound and bonded to a PP-GF30 core in the same cycle. The core material is dosed at 60–70 wt% of the total shot mass to provide structural stiffness; the remaining 30–40 wt% is the outer skin. Melt temperature for the API-2515 layer is 225–235°C, core melt at 250°C, and tool temperature at 40°C. The part is tested to ISO 6603-2 at -30°C for multiaxial puncture, ISO 527-1:2019 for tensile yield, and ISO 11359-2:2021 for thermal expansion mismatch with adjacent chrome or steel trim. UV performance is validated by SAE J2527:2017 at 2,500 kJ/m². Process failure modes include delamination at the two-material interface if the core is allowed to cool below 160°C before skin injection, and gloss variation on the step surface due to gate blush. Sequential valve gating with two center gates reduces weld line visibility; venting depth is 0.02 mm. Finished products include rear bumper step pads and bed step covers for SUVs and pickups. The operational boundary is that the EPDM-rich skin should not be placed under continuous point-load compression above 80°C; metal inserts or threaded bosses are not recommended because the rigid-tough balance is designed for clip attachment and snap mounting.
Competitive Kingfa API-2515,PP+EPDM-TD20 (Rigid-Tough Balance, UV),Automotive prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8615365186327 or mail to sales3@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8615365186327
Email: sales3@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Kingfa API-2515 is classified under ISO 1043-1 as a polypropylene compound containing an ethylene–propylene–diene monomer elastomer phase and 20 wt% talc reinforcement, designated PP+EPDM-TD20, with an ultraviolet-stabilization package intended for automotive injection-molding applications. The grade occupies a formulated position between low-density unfilled PP/EPDM impact copolymers and higher-stiffness talc-filled PP homopolymers: the talc phase increases flexural stiffness and reduces post-molding dimensional movement, while the discrete EPDM domain preserves multiaxial impact ductility at low service temperatures. The UV stabilization package extends surface integrity on semi-exterior and intermittent-sunload automotive parts such as wheel-arch liners, stone deflectors, cowl-side brackets, lower air guides, and interior load floors adjacent to glazing. Molded components produced from this compound are typically evaluated for dimensional stability after conditioning at 23°C and 50% RH for 48 h, and for mechanical response under ISO 527-2, ISO 178, and ISO 179-1/1eA. Because exact lot-specific rheological and mechanical values are subject to OEM color and stabilization adjustments, the registered Kingfa technical datasheet for API-2515 remains the controlling specification for production release.
Melt processing of API-2515 follows the shear-thinning response of a 20 wt% talc-filled impact copolymer. The barrel-temperature profile from feed to nozzle is typically maintained between 190°C and 230°C, with the actual settings adjusted to shot mass, flow-length-to-thickness ratio, and hot-runner pressure drop. Melt temperature above 230°C for extended residence time can consume the hindered-amine and phenolic stabilization package, producing pre-weathered surface embrittlement despite acceptable as-molded tensile indices. On co-rotating twin-screw compounding lines with L/D 40:1 to 48:1, the EPDM phase is introduced downstream of the PP melt zone to limit chain scission, while talc is side-stuffed into a partially filled section so that dispersive mixing occurs before the vacuum devolatilization port. Capillary rheometry per ISO 11443 should be used to develop a shear-viscosity model for gate-sizing and filling simulation; a generic PP homopolymer Cross-WLF model is insufficient because the talc platelets increase low-shear viscosity and yield stress while the EPDM domain suppresses melt fracture at high apparent shear rates.
Drying is required only when water adsorption on the talc surface exceeds normal handling limits. Under ambient conditions above 60% RH, surface moisture can generate silver streaks, splay, and reduced weld-line strength at the gate. A desiccant hopper dryer set at 80°C for 2–4 h is generally sufficient for material exposed to humid air or cold warehouse-to-molding transport. Non-desiccant hot-air drying is inadequate because water released from talc surfaces does not reach equilibrium with undried air. Mold temperatures in the 20–50°C range are typical; the upper bound improves surface replication on textured Class-B surfaces but increases cycle time. For thin-wall sections below 2.0 mm, mold temperatures near 50°C and injection velocities above 100 mm/s are commonly required to prevent short shots and free-jetting when flow length exceeds 150 mm. Hold-pressure duration should be established by gate-seal time measurement on the production tool, not transferred from unfilled PP platforms, because the mineral phase accelerates gate freeze-off and changes the shrinkage compensation window.
API-2515 is specified where a conventional talc-filled PP homopolymer would retain acceptable modulus but fail low-temperature ductility, and where an unfilled PP/EPDM impact copolymer would exhibit excessive shrinkage, lower scratch resistance, or insufficient creep resistance. The UV stabilization package is formulated to reduce the rate of photo-oxidative chain scission at the molded surface. In xenon-arc accelerated weathering per ISO 4892-2 method A or SAE J2527, UV-stabilized talc-filled PP compounds typically enter a low-gloss retention plateau before visible micro-cracking initiates in the oxidized surface layer. The talc platelets increase the tortuosity of oxygen ingress but do not eliminate oxidation; surface embrittlement will proceed if the part is used beyond the validated radiant exposure limit. Components with direct sunload, such as upper cowl grilles and wiper-washer bezels, should be validated for color shift, gloss retention, and low-temperature notched impact after accelerated weathering according to the relevant OEM weathering protocol. Published data for this specific configuration across all OEM cycles is limited; therefore end-use validation per ISO 4892-2, SAE J2527, or the corporate supply specification is required before paint-layer substitution or Class-A surface use.
Mechanical testing of API-2515 is performed on injection-molded ISO multipurpose specimens after conditioning at 23°C and 50% RH for 48 h. The EPDM phase produces a stress-whitening response at high-strain regions such as knit lines, snap-fit backwalls, and fastener bosses. Stress whitening is a ductile deformation signature; however, it may be visually unacceptable on visible surfaces without grain texture. In such cases, weld-line placement should be moved to hidden areas or gate and overflow geometry adjusted to maintain a flow-front temperature above 200°C at the knit line. The talc content reduces weld-line strength relative to bulk material; a weld-line retention factor of 0.60–0.80 is commonly observed in mineral-filled impact copolymers depending on filler orientation and melt-temperature history. Tensile elongation at break, flexural modulus, and Charpy notched impact at 23°C and −30°C should be measured on specimens cut parallel and transverse to flow to quantify orientation effects for structural brackets and snap-fit designs.
| Property | Standard designation | Specimen or test condition |
|---|---|---|
| Melt mass-flow rate | ISO 1133-1 | 230°C, 2.16 kg |
| Density | ISO 1183-1 | Immersion method, 23°C |
| Tensile properties | ISO 527-2 | Type 1A, 50 mm/min |
| Flexural modulus | ISO 178 | 2 mm/min, 23°C |
| Charpy notched impact | ISO 179-1/1eA | 23°C and −30°C |
| Heat deflection temperature | ISO 75-2 | 0.45 MPa and 1.80 MPa |
| Accelerated weathering | ISO 4892-2, SAE J2527 | Xenon-arc, gloss and color retention |
The mineral loading in API-2515 distinguishes it from adjacent PP+EPDM formulations through a shift in shrinkage anisotropy, heat deflection, and low-temperature impact. A lower-talc PP+EPDM-TD10 grade provides higher elongation at break and better knit-line strength at −30°C, but shows larger mold shrinkage, lower flexural modulus, and greater risk of sink marks over ribs and bosses. A higher-talc PP+EPDM-TD30 or TD40 grade raises flexural modulus and heat deflection temperature, but increases density, reduces melt flow, and lowers notched impact performance when the mineral phase forms continuous platelet networks at the surface. The 20 wt% plateau supplies a rigid–tough balance suitable for non-painted automotive parts that require dimensional stability, moderate thermal resistance, and practical injection-molding cycle times.
Compared with reactor TPOs or PP/EPDM blends without talc, API-2515 exhibits lower coefficient of linear thermal expansion, reduced post-molding warpage, and improved resistance to moisture-induced dimensional change. However, the mineral phase also reduces ultimate tensile elongation and increases notch sensitivity at sharp corners. Ribs, bosses, and snap arms should therefore include generous corner radii and a nominal wall-thickness-to-rib ratio consistent with PP mineral compounds; 0.6–0.8 times the adjacent wall thickness for the rib base is typical, but local flow-front and shrink compensation must be validated on the production mold. In comparison with glass-fiber-reinforced PP, the talc-filled grade has lower stiffness but produces less anisotropic warpage and lower surface fiber read-through, which is relevant for grained or low-gloss automotive surfaces.
For fastening applications, API-2515 can be used with threaded inserts, push-pin retention features, and heat-staked bosses when the local wall thickness and insertion speed are controlled. Heat staking of minerals-filled PP requires lower stake temperature and longer dwell than unfilled PP, because the talc phase increases thermal conductivity but reduces local melt flow. The grade should not be painted without adhesion validation, because the EPDM phase and talc surface chemistry affect coating wetting and surface-energy consistency. For components exposed to engine-bay cleaners, windshield washer fluid, or calcium chloride road brines, chemical compatibility should be assessed under load per the relevant OEM fluid-exposure specification. Ambient storage of molded parts or reground material above 60% RH should be avoided unless the material is re-dried before processing; the talc surface adsorbs moisture that can create splay and reduce repeatability of weld-line strength. Alkaline cleaning agents and prolonged immersion in hot glycol-water mixtures may degrade the interfacial bond between talc and the PP/EPDM matrix after sustained exposure, so chemical substitution on production parts must be validated rather than inferred from short-term immersion data.