| HS Code | 777453 |
| Material Type | PP+EPDM-TD |
| Filler Type | Talc |
| Filler Content | 20% |
| Uv Stabilization | Yes, exterior UV stabilized |
| Density | 1.04-1.06 g/cm³ |
| Melt Flow Rate | 8-15 g/10 min at 230°C/2.16 kg |
| Tensile Strength | 20-22 MPa |
| Elongation At Break | 50-100% |
| Flexural Modulus | 1600-1800 MPa |
| Notched Izod Impact Strength | 25-30 kJ/m² |
| Heat Deflection Temperature | 100-110 °C |
| Vicat Softening Temperature | 130-135 °C |
| Molding Shrinkage | 1.0-1.5% |
As an accredited Kingfa APO-2021,PP+EPDM-TD (Exterior, UV),Automotive, Structural Parts factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Kingfa APO-2021 is packed in 25 kg moisture-proof bags, 40 bags (1,000 kg) per pallet for automotive structural parts. |
| Container Loading (20′ FCL) | Kingfa APO-2021 PP+EPDM-TD UV exterior automotive structural-parts compound is loaded in a 20′ FCL container, palletized and secured for export. |
| Shipping | Kingfa APO-2021, a UV-stabilized PP+EPDM-TD automotive structural compound, ships as dry pellets in moisture-barrier bags or octabins. Transport in clean, dry, ventilated containers at ambient temperature, protected from sunlight, moisture, and contamination. Non-hazardous; use normal industrial handling and storage practices. |
| Storage | Store Kingfa APO-2021 PP+EPDM-TD compound in a cool, dry, well-ventilated warehouse. Keep in original sealed packaging on pallets, protected from direct sunlight/UV, moisture, dust, heat, ignition sources, and incompatible chemicals. Avoid outdoor storage and bag damage. Use clean handling to prevent contamination. Maintain stable ambient conditions within supplier limits, stack securely, inspect regularly, and follow first-in, first-out stock rotation. |
| Shelf Life | Typically 12 months in original sealed packaging, stored cool and dry below 30°C, away from direct sunlight and moisture. |
Injection moulding of Kingfa APO-2021 into front-end carrier tools requires pre-drying at 80°C for 3–4 h when pellet moisture exceeds 0.05 wt%; otherwise talc-bound water is released at the nozzle and produces silver streaking along the advancing melt front. The material is processed on a hydraulic clamp unit of 1,600–2,200 t with shot volume not exceeding 65–70% of barrel capacity. A screw with L/D ratio 22:1 to 25:1 and non-return valve clearance below 0.15 mm is specified to retain EPDM phase integrity during dosing. Melt temperature is held at 215–230°C, mould wall temperature at 35–50°C, and holding pressure at 45–60 MPa. Above 240°C, thermo-oxidative chain scission of the EPDM phase reduces notched Charpy impact at -30°C by 20–30%, particularly after 10–15 regrind cycles. Sequential valve-gate positioning must displace knit lines away from boss and rib feet; a fill imbalance above 5% across four hot-drop tips produces short-shot at rib terminations and anisotropic shrinkage after demoulding.
Compliance evidence for structural front-end parts includes ISO 527-2:2012 tensile yield stress, ISO 178:2019 flexural modulus, ISO 179-1:2010 notched impact at 23°C and -30°C, and ISO 75-2:2013 method B at 0.45 MPa. Vehicle-level homologation requires a production site certified to IATF 16949:2016, IMDS material data submission, and conformity to EU ELV 2000/53/EC heavy-metal limits. Flammability is demonstrated by ISO 3795:1989 or FMVSS 302 with burn rate below 100 mm/min. In terms of formulation addition, the compound is used without dry-blended filler; only closed-loop post-industrial regrind is added at 10–15 wt% for non-visible backside ribs. Terminal components include injection-moulded front-end carrier frames, radiator support end brackets, bonnet latch mounting platforms, and intercooler guide duct support ribs.
| Release parameter | Test designation | Industrial screening window for exterior PP/EPDM-talc structural compounds |
|---|---|---|
| Tensile yield stress | ISO 527-2:2012, type 1A, 50 mm/min | 17–21 MPa |
| Flexural modulus | ISO 178:2019, 2 mm/min | 1700–2300 MPa |
| Notched Charpy at -30°C | ISO 179-1:2010, 1eA | 5.5–8.5 kJ/m² |
| Heat deflection temperature | ISO 75-2:2013, method B, 0.45 MPa | 80–95°C |
| Melt flow rate | ISO 1133-1:2022, 230°C/2.16 kg | 10–18 g/10 min |
The tabulated windows are line-release screening ranges for talc-filled PP/EPDM exterior compounds; APO-2021 technical datasheet values govern final part-specific acceptance criteria. Published batch data for APO-2021 may be required when these limits are negotiated with the OEM.
Wheel arch liner production with talc-filled UV-stabilized PP/EPDM demands controlled moisture removal at 80°C for 2 h only when pellets have been exposed to RH > 60% for more than one shift. Dry-air hoppers with dew point below -30°C are preferred over recirculating compressed-air dryers because talc-filled compounds can re-adsorb moisture during conveying. The tool is a three-plate or hot-runner split-cavity mould with sequential valve gates to balance flow length ratio below 1.25. Fill velocity profiling starts at 30–40 mm/s through the gate land and rises to 80–120 mm/s after 0.3–0.5 s to prevent jetting and surface flow-marks. A nucleating or anti-scratch masterbatch is not added unless OEM grain retention testing demands it; where specified, a high-clarity carrier masterbatch is dosed at 1.5–2.5 wt%. Endothermic chemical foaming agent at 0.3–0.8 wt% can be used for weight reduction in non-visible twin-wall sections; above 1.0 wt%, the drop in notched impact at -30°C becomes statistically significant.
Qualification includes ISO 4892-2:2013 xenon-arc exposure at 0.51 W/m² at 340 nm, black-panel temperature 65°C, and 18 min spray cycles. Surface gloss retention and ΔE below OEM limits are required after 2,000–2,500 kJ/m². Multi-axial impact is measured per ISO 6603-2:2000 at -30°C, and bolt-off retention is checked after 85°C/85% RH thermal humidity cycling. The material is used at 100% virgin or with 10 wt% internal trimmings; external recycled polymer streams are excluded because unknown base-resin viscosity shifts alter flow-length reproducibility. End products are wheel arch liners, fender lower extensions, stone-guard splash shields, and air guide spoilers for front bumper undersides.
When side sill rocker panels are moulded from APO-2021, the controlling process risk is not stiffness retention but ductile-to-brittle transition shift after gas-assisted coring. Gas-channel ribs are incorporated into the B-surface so that nitrogen at 5–15 MPa penetrates the melt core after 75–85% cavity fill. The delay timer is set at 0.5–1.5 s and verified by ultrasonic wall-thickness mapping. An incorrect gas delay below 0.3 s creates fingering and uneven hollow section, reducing multi-axial impact force by 10–15% under ISO 6603-2:2000 testing at -30°C. The melt-temperature operating band is held to ±5°C around 220–230°C; mould temperature is maintained at 40–55°C. Pre-drying at 80°C for 3 h is mandatory because long flow paths expose any residual moisture to high shear at the gate land.
Exterior weathering compliance is established through SAE J2527:2017 xenon-arc exposure. Side sill parts must retain at least 70% of original Charpy notched impact after 2,500 kJ/m² with no visible chalking or microfissure. Stone-chip testing per SAE J400:2008 uses 9.5 mm gravel at 0.5 MPa air pressure on grained class-A surfaces. Chemical resistance is assessed under ISO 2812-1:2017 against road salt and automotive soap; tensile elongation retention must not fall below 80% after 48 h at 23°C. The compound is processed without external impact-modifier addition; regrind from gas-assisted sprues is limited to 8–12 wt% because gas-channel skins contain elongated talc orientation. Terminal parts include side sill claddings, lower door mouldings, rocker panel extensions, and wheel arch flare carriers with integral clip towers.
In thin-wall bumper valance and grille surround tooling, gate freeze time is governed less by shot volume than by the heat-transfer path through talc-nucleated PP/EPDM at wall thickness 2.0–2.5 mm. Melt temperature is raised to 230–235°C so that flow length reaches 250–300 mm at 2.2 mm wall without exceeding 240°C; a plateau above this limit causes EPDM thermal shearing and black specks after 20–30 shots. Gate land thickness must be 0.8–1.2 mm and gate width 4–6 mm; land length is kept below 2 mm. Mould temperature is 45–60°C, and injection velocity is profiled from 120–180 mm/s at the gate to 180–250 mm/s in the last-flow region. The packing phase uses 35–50 MPa for 0.8–1.5 s; longer packing induces overpacking at the gate and results in stress whitening near the sprue.
For molded-in-color black or dark gray exterior parts, a UV-stable masterbatch is dosed at 2.0–3.0 wt%. Doses above 3.5 wt% lower heat deflection temperature by 3–5°C under ISO 75-2:2013 method B and increase molded-in stress. Dry-blend colorants are excluded because talc-filled systems do not distribute pigment uniformly under low backpressure. Conformity of the thin-wall articles is measured by ISO 1133-1:2022 MFR at 230°C/2.16 kg for incoming resin, ISO 527-2:2012 tensile elongation at yield, and ISO 179-1:2010 notched Charpy after 85°C/85% RH humidity conditioning for 100 h. End-use parts include bumper lower valances, front grille surround frames, lower air-inlet shutters, and number-plate mounting carriers.
Tailgate lower trim and D-pillar outer cladding moulded from talc-filled UV-stabilized PP/EPDM are placed in a rear-fascia zone where rear wiper runoff, road salt, and reflected UV radiation operate simultaneously. This application uses a conventional hydraulic or servo-electric injection machine with clamp force 800–1,400 t; the screw should be a general-purpose 20:1 L/D with chromed root and screw tip because EPDM/talc compounds generate moderate screw wear. Melt temperature is held at 210–225°C, and mould temperature at 30–45°C. Drying is triggered only when granulate moisture exceeds 0.05 wt%; typical dry-air conditions are 80°C for 2–3 h. If the part is painted or film-laminated, regrind content is limited to 10 wt% to maintain consistent surface topography after VDI 3400 class-A graining at depth 12–20 µm.
In formulation terms, the visible surface is run at 100% APO-2021. A process stabilizer masterbatch may be dosed at 0.2–0.5 wt% only when extended heat aging in export shipping containers is specified. Exterior weathering is tested under SAE J2527:2017 and ISO 4892-2:2013; tailgate trim must show no dulling, cracking, or colour change ΔE > 2.0 after 1,500–2,000 kJ/m². Mechanical acceptance includes ISO 178:2019 flexural modulus before and after 30 days exterior Florida exposure; impact behaviour is measured with ISO 179-1:2010 at -30°C. End products are tailgate lower trim panels, rear bumper upper fascia covers, D-pillar outer appliqués, and rear wiper motor close-out panels.
Cowl vent grille and wiper cover parts demand a different rigidity-to-flow balance than bumper components because long unsupported spans between mounting bosses require HDT retention after underhood and outdoor heat soak. APO-2021 is injection-moulded at 220–240°C with a cold runner or hot-tip system that fills through the central rib network; flow leaders are used to avoid premature freezing at rib root thickness below 1.8 mm. Mould temperature is 40–60°C, and packing pressure is 40–60 MPa applied for 1.0–2.0 s. Insufficient packing at rib intersections produces sink marks that amplify light-reflective surface defects. Sag resistance is measured at 90°C after 1 h per OEM fixture testing, while heat deflection is characterized by ISO 75-2:2013 method B at 0.45 MPa. Weathering is tested under ISO 4892-2:2013 for 2,000 kJ/m²; the surface must retain grain and show no whitening after 10 high-pressure water jet cycles at 6 MPa.
The compound is run without filler addition. For dark molded-in-color programmes, carbon black masterbatch is added at 2.0–3.5 wt%; for painted programmes no colour concentrate is used, and the part is flame or plasma pretreated before adhesive primer application. A low-dose anti-scratch additive masterbatch at 1.5–2.5 wt% is introduced only when OEM haptic and abrasion specifications require Erichsen scratch resistance with ΔL < 1.5 after 10 cycles at 10 N. Terminal parts include cowl vent grilles, leaf screens, wiper motor covers, water deflector panels, and upper strut tower access close-outs.
In battery-electric front-trunk and charge-port applications, APO-2021 is processed at melt temperature 220–230°C and mould temperature 35–50°C on vertical or horizontal insert-moulding machines with rotary tables. Metal hinge bushings and latch bosses are inserted before moulding; differential contraction between the PP/EPDM-talc substrate and insert must be accommodated by boss wall thickness not less than 2.0 mm. Cycle time is largely set by insert conditioning at 80–100°C to avoid condensation-induced gas traps. For formulation addition, the charge-port door outer shell uses 100% virgin material; internal carrier ribs accept 10–15 wt% closed-loop regrind. Colour masterbatch is dosed at 2.0–3.0 wt% for integrated colour programmes, while painted charge-door skins are pretreated by plasma before adhesion promoter.
Compliance for these exterior structural enclosures includes ISO 527-2:2012 tensile properties, ISO 179-1:2010 Charpy impact at -40°C, and ISO 4892-2:2013 xenon-arc weathering with 1,500 kJ/m² minimum. Dimensional stability is verified after 24 h at 80°C and after 48 h water immersion at 23°C. Incompatibilities include avoidance of PA-based hinge components in direct over-moulding because differential thermal expansion above 90°C causes localised stress cracking. Terminal components are charge-port door inner and outer carriers, front-trunk gutter channels, latch striker close-outs, and structural surrounds for high-voltage service disconnect access panels.
Competitive Kingfa APO-2021,PP+EPDM-TD (Exterior, UV),Automotive, Structural Parts prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8615365186327 or mail to sales3@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8615365186327
Email: sales3@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Kingfa APO-2021, PP+EPDM-TD (Exterior, UV), Automotive, Structural Parts, is supplied as a talc-filled, EPDM-modified polypropylene compound for exterior semi-structural automotive components. The matrix is polypropylene; the impact modifier is ethylene-propylene-diene monomer; the suffix TD denotes talc filler; Exterior, UV denotes a hindered amine light stabilizer and ultraviolet absorber package. APO-2021 is not a dynamically vulcanized thermoplastic vulcanizate and does not contain short-glass reinforcement. Public lot-specific data for APO-2021 are limited; therefore the numerical ranges cited in this document are representative of 10–20 wt% talc-filled exterior PP/EPDM compounds and should be replaced by the batch release certificate for engineering calculations.
The compound is positioned for bumper support brackets, lower grille frames, rocker moldings, wheel-arch liners, and other exterior plastic structures where flexural modulus, low-shrinkage geometry, and ultraviolet resistance are specified. It is not a replacement for primary body-structure metallic components. In load-bearing applications, tensile yield stress, creep modulus, and Charpy impact data from ISO 527-2, ISO 899-1, and ISO 179-1/1eA must be used in finite-element verification rather than nominal grade designations.
Unfilled PP/EPDM blends provide high low-temperature impact but low flexural modulus. Published data for unfilled automotive PP/EPDM compounds typically show ISO 178 flexural modulus of 700–900 MPa and ISO 179-1/1eA Charpy notched impact at -40 °C of 8–12 kJ/m². Talc-filled exterior grades shift flexural modulus to approximately 1500–2200 MPa, while low-temperature impact falls to 3–6 kJ/m². Talc-only PP compounds without EPDM can exceed 2500 MPa in flexural modulus but fail brittle at low temperature; the EPDM domains in APO-2021 are retained specifically to absorb crack energy. The trade-off is therefore lower modulus than high-talc compounds but improved ductility relative to talc-only systems.
Compared with non-UV PP/EPDM-TD compounds, APO-2021 is designated for exposed exterior service because it contains the exterior stabilizer package. Non-UV talc-filled PP can develop surface chalking, gloss loss, and microcracking under xenon-arc exposure; exterior grades are formulated to delay those failure modes. APO-2021-specific weathering hours are not published in this document, so qualification against the relevant OEM weathering specification is required.
Production compounding of PP/EPDM-TD exterior grades is performed on co-rotating twin-screw extruders with L/D ratios of 40:1 to 48:1. Talc is side-fed downstream of the first mixing zones to limit platelet attrition and screw/barrel wear, while EPDM may be metered sequentially to control the dispersed-phase morphology. Vacuum venting before the discharge zone removes moisture and low-molecular-weight volatile fractions. Screw torque, vent vacuum, and melt temperature are the controlling process variables. Batch-to-batch variation in talc particle-size distribution and EPDM dispersion influences notched impact and molded-surface gloss; therefore incoming material should be tested using capillary rheometry and injection-moulded plaques, not pellet visual inspection alone.
Ultraviolet exposure degrades polypropylene by radical chain scission, causing loss of molecular weight, surface cracking, chalking, and gloss reduction. Talc filler increases the exposed mineral surface and can accelerate local surface whitening; therefore exterior talc-filled PP/EPDM grades require a light stabilizer package. APO-2021 is designated for exterior UV service and is supplied with a hindered amine light stabilizer and UV absorber package, although the full stabilizer stoichiometry is not disclosed in public documentation. Accelerated weathering performance for exterior automotive polymers is evaluated under ISO 4892-2 or SAE J2527 xenon-arc methods; gloss retention is measured according to ISO 2813 and color shift according to ASTM D2244. Published APO-2021-specific weathering exposure hours are limited; qualification against a specific OEM weathering standard is required before part approval.
Injection moulding of APO-2021 into geometrically stiff exterior parts requires control of moisture, melt temperature, and mold temperature. Talc-filled PP/EPDM compounds are not strongly hygroscopic, but surface moisture on talc can generate splay at moisture levels above 0.1 wt%, especially after storage in relative humidity above 60 %. Pre-drying at 80 °C for 2–4 h is a conservative production practice. Melt temperature at the nozzle should be maintained below 230 °C; prolonged residence time above 230 °C consumes the UV stabilizer and can shift molded color toward yellow. Starting injection moulding parameters include back pressure of 3–7 bar, screw rotation of 50–100 min⁻¹, and mold temperature from 30 °C to 70 °C. Higher mold temperature improves knit-line strength and reduces visible flow lines but increases cycle time. Clamp force requirements are typically calculated at 3–5 kN/cm² of projected area.
For exterior structural parts, the material’s combination of flexural modulus and melt flow influences wall thickness and gate placement. With melt flow rate in the 8–20 g/10 min range, flow-length-to-wall-thickness ratios up to 200:1 are feasible in uniform-wall designs. Abrupt thickness changes and sharp corners produce knit lines and low-temperature fracture sites because talc platelets orient along the flow front. Ribs should be limited to 60 % of nominal wall and corners should be radiused to at least 1.0 mm in impact-loaded regions.
The design window is bounded by low-temperature brittleness and high-temperature creep. At -40 °C, talc-filled PP/EPDM parts can fracture at weld lines, gate vestiges, and sharp radii; if Charpy notched impact values are below 5 kJ/m², additional radius, wall thickening, or gate relocation is necessary. At service temperatures approaching 90 °C, the same component may lose clamp retention in snap-fit features because creep modulus under load decreases; ISO 899-1 tensile creep data should be used for permanent set calculations. Talc orientation during mold filling produces anisotropic shrinkage and can generate warpage in long thin sections. The higher flexural modulus of APO-2021 relative to unfilled PP/EPDM permits thinner wall sections, but only when the shut-off and rib ratios are adjusted for talc’s reduced ductility.
Compared with short-glass polypropylene structural grades, a 20 wt% talc-filled PP/EPDM compound has lower density and lower flexural modulus. Short-glass PP grades typically exhibit flexural modulus of 3000–4000 MPa and density near 1.12–1.14 g/cm³, whereas talc-filled exterior PP/EPDM compounds are in the 1.03–1.08 g/cm³ density range and 1500–2200 MPa flexural modulus range. The talc system gives lower warpage and better surface appearance than short glass, but it cannot carry the same sustained structural load. This distinction matters in exterior semi-structural parts that must combine dimensional stability with pedestrian impact and cold-impact ductility.
Representative property envelope for 10–20 wt% talc-filled exterior PP/EPDM compounds; APO-2021-specific release data should be used for final part sign-off.
| Property | Test method | Representative range | Notes |
|---|---|---|---|
| Density | ISO 1183-1:2019 | 1.03–1.08 g/cm³ | Filler loading affects part mass. |
| Melt flow rate, 230 °C/2.16 kg | ISO 1133-1:2022 | 8–20 g/10 min | Higher values ease filling but may reduce impact. |
| Tensile stress at yield | ISO 527-2:2012 | 17–23 MPa | Use as lower-bound for short-term load. |
| Tensile elongation at break | ISO 527-2:2012 | 50–150 % | Higher EPDM increases ductility. |
| Flexural modulus | ISO 178:2019 | 1500–2200 MPa | Governs snap-fit and bracket stiffness. |
| Charpy notched impact, 23 °C | ISO 179-1:2010 | 15–35 kJ/m² | Moulded plaque value; part geometry reduces service energy absorption. |
| Charpy notched impact, -40 °C | ISO 179-1:2010 | 3–6 kJ/m² | Critical for cold-impact exterior parts. |
| Heat deflection temperature, 0.45 MPa | ISO 75-2:2013 | 95–115 °C | Not a continuous use temperature. |
| CLTE, -30 °C to 80 °C | ISO 11359-2:2021 | 60–90 µm/m·°C | Lower than unfilled PP but higher than short-glass PP. |
| Mould shrinkage, parallel | ISO 294-4:2018 | 0.7–1.0 % | Anisotropic; gate location controls warpage. |
For production release, APO-2021 should be controlled by a batch release certificate that includes actual melt flow rate, filler content, tensile, flexural, and impact data. Automotive IMDS submission requires full substance declaration; alteration in stabilizer package or talc source between campaigns may affect material classification.
| Standard or directive | Scope | Application to APO-2021 |
|---|---|---|
| ISO 4892-2 / SAE J2527 | Xenon-arc weathering | Exterior UV durability validation. |
| ISO 527-2 / ISO 178 | Mechanical properties | Part design and structural calculation. |
| ISO 179-1/1eA | Charpy notched impact | Low-temperature toughness validation. |
| REACH 1907/2006 | SVHC declaration | EU supply; confirm from supplier SDS/CoA. |
| RoHS 2011/65/EU | Restricted heavy metals | May be requested for electrical/electronic subcomponents; not default automotive requirement. |
| IMDS Recommendation 001 | Material data reporting | OEM part approval and substance tracking. |
In painted exterior parts, talc-filled PP/EPDM surfaces require adhesion promoters based on chlorinated polyolefins or flame/plasma surface activation. The talc/mineral layer can concentrate near the surface and reduce paint adhesion if mold temperature is too low or if the melt front shears excessively. Adhesion testing may follow ISO 2409 cross-cut or OEM stone-chip tests. For molded-in-color applications, the UV package should be validated for color shift and gloss retention under the full exterior weathering specification.
Avoid deliberate addition of peroxide masterbatches or amine-based additives to APO-2021 unless validated by capillary rheometry and weathering data; amine residues can neutralize the acid-scavenging stabilizer and accelerate UV yellowing. The compound is not designed for sustained contact with aggressive brake fluid or battery acid. Continuous service under load above 100 °C is outside the expected operational envelope. High-shear processing above 240 °C or residence time beyond 10 min can cause thermal degradation of both PP and EPDM and should trigger purge protocols.