| HS Code | 575424 |
| Base Polymer | Polypropylene (PP) |
| Elastomer Modifier | EPDM |
| Filler Type | Talc |
| Uv Stabilization | Yes |
| Molding Shrinkage Percent | 0.8-1.2 |
| Processing Method | Injection molding |
As an accredited Kingfa APO-3006,PP+EPDM-TD30,Automotive,Exterior, UV factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Kingfa APO-3006 PP+EPDM-TD30 automotive exterior UV compound is packaged in 25 kg moisture-resistant bags, 40 bags per pallet. |
| Container Loading (20′ FCL) | 20′ FCL: palletized 25 kg bags of Kingfa APO-3006 PP+EPDM-TD30 automotive exterior UV compound, loaded dry under ambient conditions. |
| Shipping | Shipping description: Non-hazardous polypropylene compound pellets, Kingfa APO-3006 (PP+EPDM-TD30, UV-stabilized automotive exterior grade). Supplied in 25 kg moisture-barrier bags or 500–1000 kg FIBCs. Transport in dry, clean trucks/containers; protect from sunlight, moisture, contamination, and excessive heat. No dangerous goods classification; store sealed, cool, and dry. |
| Storage | Store Kingfa APO-3006 in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, moisture, and open flames. Keep original sealed packaging on pallets, protected from UV exposure and contamination. Avoid outdoor storage and extreme temperatures. Maintain stable conditions, good stacking, stock rotation, and inspect packages regularly for damage. Follow supplier shelf-life and storage recommendations. |
| Shelf Life | Shelf life is typically two years when stored dry, in original sealed packaging, away from direct sunlight, heat, and moisture. |
In front-end lower grille and radiator grille surround moulding, APO-3006 is processed as a 30 wt% talc-filled PP/EPDM compound at a formulation addition ratio of 100 wt% available material, with injection-grade regrind from the same part family limited to 20 wt% because repeated heat history reduces the EPDM phase’s ability to absorb impact energy at -30 °C. When colour adjustment is not supplied as pre-coloured compound, 2–3 wt% carbon-black PP-based masterbatch is dosed at the feed throat. Actual lot melt flow is verified per ISO 1133-1:2022 at 230 °C with 2.16 kg load before job startup; talc moisture and EPDM-phase crosslink history can shift MFR by 2–4 g/10 min across batches. Compliance for unpainted exterior grille surfaces references ISO 4892-2:2013 Method A Cycle 1 and SAE J2527 at 1,000–1,500 kJ/m² cumulative irradiance; flammability is controlled to FMVSS 302 / SAE J369 horizontal burn criteria, and chemical registration is maintained under REACH Regulation (EC) No 1907/2006 and the ELV Directive 2000/53/EC heavy-metal restrictions. Processing on production-scale injection machines with 22:1–25:1 L/D plasticating units requires nozzle melt temperature of 230–250 °C, mould-surface temperature of 30–50 °C, and hydraulic holding pressure of 45–65 MPa. Because the talc fraction abrades non-return valve lands, shot-weight drift of 1.5–3.0% is observed after approximately 20,000 cycles unless the check ring is inspected and replaced. Multi-gate sequencing shifts weld lines to the lower grille perimeter away from snap-fit posts; pack time is maintained at 8–15 s until gate freeze is verified by part-weight stability. Terminal product types include front bumper lower grilles, radiator grille surrounds, front fascia close-out panels, and tow-hook covers.
The primary failure mode in wheel arch liner production is brittle cracking at the mounting flange when cold-impact energy is localized at clip towers. APO-3006 is moulded at a formulation ratio of 80 wt% virgin compound to 20 wt% dried TPO production regrind, with 2.0–2.5 wt% black colour masterbatch added only if the lot is non-precoloured; higher filler or regrind levels reduce ISO 179-1:2020 notched Charpy impact below 18 kJ/m² at -30 °C. Compliance for wheel arch liners references ISO 6603-2 for multiaxial impact, ISO 4892-2:2013 xenon-arc weathering at 1,200 kJ/m², and FMVSS 302 for burn resistance. Injection moulding is conducted on clamp force platforms of 1,200–1,600 t because projected part area can exceed 0.6 m². Melt temperature is kept at 235–250 °C, while mould temperature is controlled at 25–40 °C with water/glycol channels positioned to avoid over-cooling textured ribs. Flow length from the sprue to the last fastener boss is reduced by using 4–6 heated valve-gated drops; when the flow path exceeds 600 mm, injection speed is raised to 30–50 mm/s ram velocity to prevent early freeze of the talc-filled melt front. Terminal product types include front wheel arch liners, rear wheel arch liners, fender splash shields, and wheel-house close-out extensions used without post-mould painting.
Under the cowl panel water-management load case, APO-3006 is processed neat at a 100 wt% addition ratio, with in-house regrind held to 10 wt% when a visible Class A surface is specified because talc-rich regrind produces silver streaks at hot-runner junctions. The dominant processing conflict is balancing high flow length with low residual stress: melt temperature at the nozzle is set to 225–245 °C, and the mould surface is run at 30–45 °C to limit warpage in ribs that form water troughs. Published mould-flow data for APO-3006 in gas-assisted cowl grille configurations is limited, so gate location and pack pressure are established on tool trials using cavity pressure sensors set to trigger transfer at 55–70 MPa. Compliance references ISO 178:2019 flexural modulus for structural channel stiffness, ISO 4892-2:2013 weathering at 1,000 kJ/m² for unpainted black surfaces, FMVSS 302 for firewall-adjacent flammability, and UN ECE R26 for external projections on wiper arm pivot surrounds. After demoulding, parts are routed to automated deflashing of living-hinge slots and then to thermal staking of rubber seals; the talc-filled compound must retain ductility at the living hinge, which is evaluated by bending the hinge through 180° at -20 °C without visible surface cracking. Terminal product types include windshield cowl grilles, plenum chamber close-outs, wiper motor covers, and lower windshield garnish mouldings.
B-pillar appliqué sections with rib bosses located on the B-surface are assessed for sink-mark depth because the 30 wt% talc phase in APO-3006 lowers bulk shrinkage but also increases orientation-driven differential shrinkage between flow and cross-flow directions. The component is formulated at 100 wt% APO-3006, with regrind limited to 10 wt% and black UV-stabilized masterbatch at 2 wt% only when moulded as a textured exterior surface. Compliance for such exterior vertical panels is driven by ISO 527-2 tensile elongation retention after weathering, ISO 178:2019 flexural modulus for edge-stiffness, and SAE J2527 for 1,500 kJ/m² exterior colour retention without blooming of EPDM stabilizers. Injection moulding parameters for sink mitigation use a high-flow profile: nozzle melt temperature 220–235 °C, mould temperature 40–50 °C, and holding pressure 55–70 MPa applied for 10–20 s depending on boss wall thickness. The holding pressure must be maintained until the gate freezes; premature release of hold pressure at 6 s is associated with sink depths exceeding 0.02 mm over screw bosses. Venting at the last-filled textured edge is cut to 0.015–0.030 mm to prevent gas burn while maintaining flow front pressure. Terminal product types include black B-pillar appliqués, C-pillar exterior trims, door beltline mouldings, and quarter-glass garnish covers.
Across a rocker panel length of 1.4–1.8 m, sequential valve gating creates multiple flow-front interruptions where talc particles orient perpendicular to flow, weakening melt-line tensile strength. APO-3006 is introduced at a formulation ratio of 95 wt% virgin compound with 5 wt% clean in-house PP/EPDM regrind; no additional filler is permitted because talc already accounts for 30 wt% of the compound and higher effective filler loading accelerates clip-boss stress cracking. Compliance for rocker panel mouldings is referenced to ISO 179-1:2020 notched Charpy at -30 °C, ISO 6603-2 multiaxial impact at 2.4 m/s striker velocity, FMVSS 302, and UN ECE R26 external projection requirements for sill edges. Moulding is performed on 1,200–1,800 t injection presses with L/D ratios of 22:1–25:1, using nozzle melt temperature 230–250 °C and cooling channel temperature 35–50 °C. Valve gate open sequence is programmed to fill the centre section first and then advance outward so that the melt line is relocated to the lower edge outside the clip-boss load path; part warpage is limited to 1.5 mm over the package length by asymmetric cooling on the B-surface. Clip bosses with root wall thickness 1.2–1.5 times the nominal wall require hold pressure of 50–65 MPa to avoid void formation. Terminal product types include painted rocker panel mouldings, side sill garnishes, lower door claddings, and rear bumper side extensions.
When APO-3006 is moulded into exterior mirror housing lower shells, the talc-filled TPO phase reduces the need for post-mould painting but imposes stricter dimensional tolerance control because mineral-filled PP/EPDM exhibits higher thermal expansion than glass-filled ABS and lower moisture uptake. The formulation addition ratio is 100 wt% APO-3006 for lower shells, with regrind limited to 15 wt% only in non-appearance inner shells; UV resistance is supplied by the compound package and verified under ISO 4892-2:2013 at 1,200 kJ/m² and SAE J2527 with ΔE ≤ 3.0. Compliance additionally references ISO 527-2 tensile properties, ISO 179-1:2020 notched impact at -30 °C, RoHS Directive 2011/65/EU, and ELV Directive 2000/53/EC. Moulding equipment for mirror shells uses 150–300 t clamp force because the projected area per cavity is small but the wall thickness drops to 1.5–1.8 mm at the shell rim. Melt temperature at the nozzle is held at 235–245 °C, mould temperature at 40–50 °C, and injection speed at 25–45 mm/s; holding pressure of 45–65 MPa is required to prevent sink at the mirror pivot boss. The talc particles increase wear on hot-tip gates, observed as gate-stringing after 15,000–20,000 cycles when gate land clearance exceeds 0.05 mm. Terminal product types include exterior mirror lower shells, mirror bezels, mirror base covers, and signal lamp retainer brackets.
Competitive Kingfa APO-3006,PP+EPDM-TD30,Automotive,Exterior, UV prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8615365186327 or mail to sales3@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8615365186327
Email: sales3@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Kingfa APO-3006 belongs to the PP+EPDM-TD30 family, a polypropylene matrix modified with an ethylene-propylene-diene monomer impact modifier and a talc reinforcement phase at a nominal loading of 30% by weight. The grade is positioned for unpainted exterior automotive components in which long-term UV stability, low-temperature ductility, and reduced post-mold warpage are functional requirements rather than secondary properties. Published data for this specific configuration is limited; the processing and performance envelope described here should therefore be treated as the intersection of Kingfa application guidance and measured behavior for PP+EPDM-TD30 systems evaluated under ISO and ASTM methods.
The primary use cases are exterior trim parts that must survive direct sun exposure without paint: lower bumper inserts, rocker panel moldings, wheel arch liners, and cowl covers. In these applications the material is typically textured to hide flow marks and scratch damage. The UV package is compounded into the pellet rather than applied as a coating, which eliminates post-molding painting but limits the achievable gloss and color match compared with painted mineral-filled PP. This distinction matters when adjacent body panels are painted class A surfaces; APO-3006 is not formulated for direct topcoat adhesion without surface treatment.
Relative to unfilled PP homopolymer, the talc reduces average mold shrinkage from above 1.2% to a flow-direction value near 0.6–1.0% and raises flexural modulus into the 1600–2100 MPa band. Relative to unfilled PP/EPDM TPO, the talc provides lower CLTE and better scratch resistance, but it also lowers -30°C notched impact energy because rigid inclusions concentrate stress at the EPDM-matrix interface. The result is a balance between dimensional stability and low-temperature ductility that is appropriate for exterior trim but not for underbody impact structures.
Under impact loading, the EPDM domains act as cavitation sites. When a crack front encounters an elastomer particle, local triaxial stress causes void nucleation at the elastomer-matrix interface; the void growth absorbs energy and blunts the crack tip. In talc-filled systems, however, the talc platelets create additional stress concentrations and reduce the distance between cavitation sites. The practical consequence is that PP+EPDM-TD30 retains ductile behavior at room temperature but undergoes a pronounced ductile-brittle transition between 0°C and -20°C, depending on EPDM content and rubber particle size distribution.
Representative Charpy notched impact values for this product category under ISO 179-1:2010 are 25–50 kJ/m² at 23°C and 3–6 kJ/m² at -30°C. The wide range reflects differences in injection speed, melt temperature, and gate geometry during specimen preparation. Because the EPDM phase is shear-sensitive, high melt temperatures above 250°C can lower impact energy by degrading the rubber crosslinks, while low melt temperatures below 210°C can leave talc agglomerates that initiate premature fracture. Production technicians should monitor barrel temperature profiles and use a melt pyrometer to confirm actual melt temperature within ±5°C of the approved process sheet.
For exterior parts that receive multiple impacts from road debris, the more relevant method is multiaxial puncture. Testing under ISO 6603-2:2000 at -20°C on 2 mm injection-molded plaques frequently discriminates between lots that pass Charpy but crack on vehicle. A lot that exhibits excessive micro-porosity from moisture or gas entrapment will show puncture energy scatter exceeding 15% of the mean, which is an early indication of surface delamination under stone impact.
MFR testing under ISO 1133-1:2022 at 230°C and 2.16 kg generally places PP+EPDM-TD30 products in the 10–20 g/10 min range. The shear-thinning behavior is dominated by talc particle alignment and EPDM droplet elongation. In thin-wall exterior parts with flow lengths above 400 mm, a melt temperature of 230°C to 240°C and a mold temperature of 30°C to 60°C are typical. Slow injection speeds produce visible flow hesitation at the gate and can reduce surface texture replication; high speeds above 200 mm/s can generate shear heating sufficient to degrade the EPDM phase unless the screw tip is equipped with a temperature probe.
Pre-drying is required when material has been exposed to ambient humidity above 60% RH for more than 4 h. The recommended drying condition is 80°C for 2–4 h in a desiccant dryer with a dew point below -20°C. Moisture contents above 0.05% appear as splay on textured surfaces and lower weld-line strength. Because talc is hygroscopic and EPDM slows moisture diffusion, simple hopper dryers are not sufficient for regrind streams above 20% recycled content.
Mold shrinkage under ISO 294-4:2018 is anisotropic: flow-direction shrinkage is lower than cross-flow shrinkage because talc platelets align during filling. The typical flow-direction band is 0.6–1.0%, while cross-flow can reach 0.7–1.1%. Shrinkage variation across a tool face is the main source of warpage in long rocker panels. Tools should use multiple gates or sequential valve gating to maintain a uniform packing pressure profile; otherwise the glass-fiber-like orientation of talc near the gate creates a local shrinkage gradient that cannot be corrected by increasing hold pressure alone.
Weathering qualification for exterior PP+EPDM-TD30 compounds is typically performed under xenon-arc exposure following SAE J2527 or ISO 4892-2:2013 cycle 1. The UV stabilizer package in APO-3006 is formulated for long-term retention of surface gloss and color; however, published data for this specific configuration is limited. In the general product category, an acceptance window of ΔE ≤3.0 and gloss retention above 60% after 1500 kJ/m² is common for exterior trim specifications, though darker color concentrates may reach higher surface temperatures and should be tested to higher radiant exposure. Test panels should be textured to match production surfaces because smooth plaques weather differently than grained surfaces.
The stabilizer package creates an operational boundary: APO-3006 should not be reprocessed more than two additional heat histories beyond the original pellet and first molded part because the hindered amine light stabilizer component is partially consumed during each high-shear extrusion cycle. Accumulation of regrind above 30% can reduce UV resistance by depleting the surface stabilizer concentration. Additionally, the grade is not recommended for continuous contact with aromatic hydrocarbons, strong oxidizing acids, or polyvinyl chloride plasticizer systems because these agents can extract the EPDM phase or attack the talc-matrix interface.
Compared with interior UV-stabilized PP compounds, exterior APO-3006 uses a heavier stabilizer loading and a more thermally stable EPDM grade. Interior grades may use lower-cost phenolic antioxidants and are not required to withstand wet-dry cycling under UV; transferring an interior PP/EPDM-TD grade to an exterior lower fascia often results in chalking and gloss loss within 12 months of Florida exposure.
Exterior trim modules are rarely made from a single material. APO-3006 parts are commonly assembled with integral clips, heat-staked bosses, or co-molded seals. The thermal expansion mismatch between the talc-filled PP matrix and attached steel or rigid thermoplastic fasteners creates stress during temperature cycling. The linear coefficient of thermal expansion for PP+EPDM-TD30 measured under ISO 11359-2:2021 is typically 60–90 µm/m·K in the flow direction and 80–110 µm/m·K across flow, substantially lower than unfilled PP but still higher than steel at 12 µm/m·K. Fastener locations must allow sliding clearance to avoid buckling at summer cabin soak temperatures above 80°C.
Molded bosses in APO-3006 can crack if the screw insertion speed is too high; the talc orientation around the boss creates a weak plane perpendicular to the flow direction. Production-scale experience with analogous grades indicates that bosses should have a minimum outside diameter of 2× the screw major diameter and a wall thickness not less than 1.5 mm to resist hoop stress. Ultrasonic welding is generally not recommended because the talc reduces energy transmission at the joint; vibration welding or hot-plate welding is preferred for joining PP+EPDM-TD30 to itself.
The following test methods are used for PPAP and annual re-qualification of exterior PP+EPDM-TD30 materials. Specific lot results for APO-3006 should be obtained from the supplier certificate of analysis, since nominal values can shift with color concentrate and regrind level.
| Property | Method | Typical Acceptance Band | Notes |
|---|---|---|---|
| Density | ISO 1183-1:2019 | 1.10–1.14 g/cm³ | Colorant affects density |
| Melt flow rate | ISO 1133-1:2022 | 10–20 g/10 min | 230°C, 2.16 kg |
| Tensile stress at yield | ISO 527-2:2012 | 18–23 MPa | Type 1A, 50 mm/min |
| Tensile strain at break | ISO 527-2:2012 | 60–150% | Thickness 4 mm |
| Flexural modulus | ISO 178:2019 | 1600–2100 MPa | 2 mm/min |
| Charpy notched impact 23°C | ISO 179-1:2010 | 25–50 kJ/m² | Edgewise, type A |
| Charpy notched impact -30°C | ISO 179-1:2010 | 3–6 kJ/m² | Conditioned 24 h |
| HDT 0.45 MPa | ISO 75-2:2013 | 95–110°C | Flatwise |
| Mold shrinkage flow/cross | ISO 294-4:2018 | 0.6–1.0% / 0.7–1.1% | Textured plaque |
| CLTE flow/cross | ISO 11359-2:2021 | 60–90 / 80–110 µm/m·K | -30°C to 80°C |
In compound selection, APO-3006 occupies a middle point between PP+EPDM-TD20 and PP+EPDM-TD40. A TD20 grade provides higher impact and easier flow but lower stiffness and greater shrinkage; a TD40 grade provides higher flexural modulus and lower CLTE but reduces weld-line strength and makes low-temperature ductility marginal. The 30% talc loading in APO-3006 is therefore not arbitrary: it is the typical compromise for unpainted exterior trims where warpage control and stone-impact toughness must be met without secondary painting.
Compared with talc-free PP/EPDM reactor blends, APO-3006 shows higher modulus and lower surface tack, which improves dirt release and scratch visibility. However, talc-free TPOs generally outperform TD30 grades in -40°C impact and hinge or snap-fit applications. APO-3006 is therefore not recommended for living hinges or snap-fit clips that must survive multiple flexural cycles at subzero temperatures.
Compared with 20% glass-fiber reinforced PP for exterior brackets, APO-3006 has lower anisotropy, lower warpage, and better surface appearance, but it cannot match the tensile modulus or creep resistance of glass-filled PP. If the part must bear constant load at temperatures above 80°C, a glass-filled grade should be evaluated; the talc-filled EPDM system will creep more and lose fastener torque retention. Back pressure during screw recovery should be limited to 4–8 bar hydraulic. Higher back pressure can increase melt temperature and degrade EPDM. Screw speeds above 120 rpm on a 60 mm general-purpose screw may generate enough shear heating to push melt temperature beyond the recommended ceiling.
Suitable wall thickness for APO-3006 exterior trim is 1.5–3.5 mm. Below 1.5 mm, talc orientation creates brittle behavior at knit lines; above 3.5 mm, sink marks and void formation increase because the semicrystalline matrix shrinks more than the talc phase allows. Rib-to-wall ratio should not exceed 0.6 to avoid sink on textured surfaces.