| HS Code | 681527 |
| Polymer Type | Polypropylene Copolymer |
| Filler Type | Mineral Filled |
| Density | 1.05 g/cm³ |
| Melt Flow Rate | 8.0 g/10 min (230°C/2.16 kg) |
| Tensile Strength | 25 MPa |
| Tensile Elongation At Break | 20% |
| Flexural Modulus | 1800 MPa |
| Notched Izod Impact Strength | 4.0 kJ/m² at 23°C |
| Heat Deflection Temperature | 100°C at 0.45 MPa |
| Molding Shrinkage | 1.2% |
| Flammability | HB |
As an accredited Kingfa PP-92010,PP Copolymer,Home Appliance, Mineral Filled factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Kingfa PP-92010 mineral-filled PP copolymer for home appliances is packed in 25 kg moisture-proof paper sacks on pallets. |
| Container Loading (20′ FCL) | Kingfa PP-92010 mineral-filled PP copolymer for home appliances loaded in a 20′ FCL container, palletized and secured for export shipment. |
| Shipping | Kingfa PP-92010 is shipped as a non-hazardous, mineral-filled PP copolymer in moisture-resistant bags or octabins. Store in a dry, ventilated area away from direct sunlight and heat. Handle with standard industrial precautions; no special transport classification is required. Keep sealed until use and protect from moisture and contamination during transport. |
| Storage | For Kingfa PP-92010 (PP copolymer, mineral filled), store in a cool, dry, well-ventilated area away from direct sunlight, heat, flames, and ignition sources. Keep original packaging sealed and clearly labeled; protect from moisture, dust, oils, and contamination. Stack pallets securely without excessive load or deformation. Avoid contact with strong oxidizers and follow local storage regulations. |
| Shelf Life | Typically 12–24 months in original unopened packaging, stored dry and cool, protected from moisture, heat, and UV. |
In front-loading washing machine detergent dispenser housings and top cover frames, Kingfa PP-92010 is processed as a compounded mineral-filled PP copolymer without further addition of filler at the molding machine. When regrind is incorporated, the ratio is held between 15 wt% and 20 wt% regrind to virgin compound to limit shifts in melt viscosity and filler distribution; higher regrind fractions have produced inconsistent cushion-rib fill in multi-cavity tools. The melt temperature is set between 220 °C and 240 °C, the mold temperature between 30 °C and 50 °C, and hydraulic hold pressure between 60 MPa and 70 MPa. Drying is not required under normal indoor storage below 60% RH, but 2 h at 80 °C is used when surface condensation is observed. Injection speed is set to maintain a melt front velocity of 150 mm/s to 250 mm/s; above 300 mm/s, visible gate blush on textured surfaces is a recorded failure mode on 1,800 kN machines using 45 mm diameter screws with 20:1 L/D. Detergent drawer components are qualified under IEC 60335-1:2020 clause 30.1 ball pressure testing at 125 °C for external thermoplastics and under IEC 60335-2-7 for washing machines. The final parts are detergent dispenser housings, top cover frames, and lid trim, where the copolymer phase improves resistance to stress cracking caused by sodium alkylbenzene sulfonate detergents compared with homopolymer PP. Because published data for this specific Kingfa grade configuration is limited, converters commonly pre-qualify with an in-house 500 h soak at 70 °C in a 5 g/L anionic detergent solution and monitor visual stress crack initiation at screw bosses and weld lines.
Refrigerator air duct frames and evaporator covers use a filler loading in the lower half of the appliance range, typically 15 wt% to 18 wt%, to balance flexural modulus and sub-zero impact after the part is mounted inside a freezer compartment. At 20 wt% filler, the linear coefficient of thermal expansion of a mineral-filled PP copolymer is often between 40 µm/m·K and 60 µm/m·K when tested under ISO 11359-2:2021, compared with 90 µm/m·K to 110 µm/m·K for unfilled PP. The injection mold is designed with a central edge gate feeding a 2.5 mm nominal wall; wall thickness below 2.0 mm has caused short shots in evaporator cover ribs when melt temperature drops below 210 °C. Processing uses a melt temperature of 210 °C to 230 °C, mold temperature of 30 °C to 40 °C, and packing pressure of 55 MPa to 65 MPa for 5 s to 8 s, followed by a hold time of 15 s to 20 s. Dimensional checks after molding are performed at 23 °C and 50% RH after 48 h conditioning. Compliance for refrigerator air ducts is not food contact; electrical safety applies under IEC 60335-2-24:2022 and fire resistance under IEC 60335-1:2020 clause 30.2 for parts in contact with live connections if the duct carries an evaporator fan harness. The final parts include evaporator cover frames, cold air duct panels, and shelf rail brackets, where the mineral filler limits post-mold warpage caused by asymmetric cooling. A production-line failure mode observed on multi-cavity tools is differential flange bending when the fixed and movable mold sides differ by more than 10 °C; maintaining coolant circuits within 5 °C across the mold faces reduces this defect to acceptable levels.
The following ranges are representative for appliance-grade mineral-filled PP copolymers with 12 wt% to 25 wt% mineral filler. They are not grade-specific release data.
| Property | Test method | Representative range |
|---|---|---|
| Melt mass-flow rate | ISO 1133-1:2022, 230 °C, 2.16 kg | 12–25 g/10 min |
| Density | ISO 1183-1:2019 | 1.04–1.08 g/cm³ |
| Tensile yield stress | ISO 527-2:2012 | 22–28 MPa |
| Flexural modulus | ISO 178:2019 | 1,800–2,800 MPa |
| Charpy notched impact strength | ISO 179-1:2010, 23 °C | 2.0–5.0 kJ/m² |
| Heat deflection temperature | ISO 75-2:2013 method B, 0.45 MPa | 100–120 °C |
| CLTE | ISO 11359-2:2021 | 40–70 µm/m·K |
Dishwasher lower spray arms and filter screens are molded with a mineral filler fraction between 15 wt% and 20 wt%; the lower end is preferred when the spray arm has a through-bore and two opposing weld lines. A higher filler fraction above 22 wt% reduces weld line impact resistance under ISO 179-1:2010 Charpy notched testing at 23 °C, with failure at the weld line recorded before bulk yielding. The processing window uses a melt temperature of 230 °C to 250 °C, a mold temperature of 40 °C to 60 °C, and a fill time of 1.5 s to 2.5 s to prevent flow hesitation behind the central core. Solid spray arms with an internal water channel are formed by a hydraulic slide core with a 3.0 mm ± 0.2 mm nominal wall; the slide is retracted after packing pressure of 50 MPa to 60 MPa is released. Drying is applied at 80 °C for 2 h to 3 h whenever storage RH exceeds 60%, because surface moisture on mineral filler can generate splay at gate exits. Wet chemical exposure is evaluated under ISO 175 using deionized water at 85 °C with 2 mg/kg active chlorine for 1,000 h; tensile strength retention above 80% is expected for copolymer grades, but converters must verify because published data for this specific configuration is limited. Final parts include lower spray arms, upper spray arm connectors, and filter screen frames. Compliance is governed by IEC 60335-2-5:2012 for dishwashers and IEC 60335-1:2020 clause 30.1 ball pressure at 125 °C for parts adjacent to the heating element in pump housings.
High-gloss air conditioner front panels molded from mineral-filled PP copolymer are constrained by a direct conflict between surface appearance and dimensional stability. Filler loading is kept between 12 wt% and 15 wt% because higher mineral fractions above 18 wt% produce surface micro-roughness that lowers 20° gloss below 80 GU on an SPI-A2 polished mold. To compensate for the lower filler content, the machine is configured with a packing pressure of 70 MPa to 90 MPa and a screw forward time of 6 s to 10 s. Melt temperature is 230 °C to 250 °C, mold temperature is 40 °C to 60 °C, and the injection speed is segmented: the first 60% of flow length is filled at 40 mm/s to 60 mm/s ram speed, and the remaining 40% is reduced to 20 mm/s to 30 mm/s to prevent gate blush. The molding machine uses a 45 mm three-zone screw with 20:1 L/D and a non-return valve with a 45° sliding angle; worn check rings are a known source of cushion variation and sink marks around bosses. Compliance for indoor air conditioner panels includes IEC 60335-2-40:2022, and external thermoplastic parts are tested under IEC 60335-1:2020 clause 30.1 ball pressure at 75 °C to 125 °C depending on proximity to the heat exchanger. Flame retardance is usually not required for indoor panels; if the panel is near live parts, a glow wire test at 650 °C under IEC 60695-2-11 is applied. Final parts include front panels, air guide louvers, and filter access covers, where low warpage after 48 h conditioning is controlled by mold temperature uniformity and balanced gate positions.
| Application segment | Relevant standard | Test or clause |
|---|---|---|
| Washing machine detergent housing | IEC 60335-1:2020, IEC 60335-2-7 | Ball pressure 125 °C; glow wire if live part |
| Refrigerator air duct | IEC 60335-2-24:2022 | Clause 30.2 fire; ISO 11359-2:2021 CLTE |
| Dishwasher spray arm | IEC 60335-2-5:2012 | ISO 175 hot water/chlorine exposure |
| Air conditioner front panel | IEC 60335-2-40:2022 | IEC 60695-2-11 glow wire 650 °C |
| Microwave door bracket | IEC 60335-2-25:2010 | IEC 60335-1:2020 clause 30.2 glow wire 750 °C |
| Rice cooker hinge bracket | IEC 60335-2-15:2012 | Ball pressure 125 °C; FDA 21 CFR 177.1520 if indirect contact |
| Vacuum cleaner floor nozzle | IEC 60335-2-2:2009 | ISO 180:2019 Izod at 23 °C and -10 °C |
On microwave oven assembly lines, door inner frames and control panel brackets are injection molded with a mineral filler fraction of 18 wt% to 22 wt% to prevent deflection when the door hinge spring is secured. The material is dried at 80 °C for 2 h only if storage RH has exceeded 60%; otherwise process stability on a 1,800 kN machine is sufficient with virgin granulate. Melt temperature is set between 220 °C and 240 °C, mold temperature between 35 °C and 50 °C, and screw back pressure between 0.5 MPa and 1.0 MPa. The door inner frame is not placed inside the microwave cavity where high flame resistance is needed; it is a mechanical carrier outside the cavity, so UL 94 HB is generally acceptable. Compliance for the appliance is based on IEC 60335-2-25:2010 and IEC 60335-1:2020 clause 30.2 glow wire end-product testing at 750 °C for connections carrying current above 0.5 A, not on the polymer alone. Final parts include door inner frames, control panel mounting brackets, and door handle bases. A production bottleneck seen with filled PP in these multi-boss parts is sink marks on the opposite face when boss thickness exceeds 60% of the nominal wall; the mold maker should core the boss rather than increasing packing pressure beyond 80 MPa.
Because rice cooker hinge brackets and steam valve retainers are exposed to steam during the cooking cycle, a higher mineral filler fraction from 20 wt% to 25 wt% is used to hold heat deflection temperature above 105 °C at 0.45 MPa under ISO 75-2:2013 method B. The processing window is narrower than refrigerator parts because the thick hinge boss and thin steam vent wall trigger differential shrinkage when the packing phase is too short. Melt temperature is set at 230 °C to 250 °C, mold temperature at 50 °C to 65 °C, and holding pressure at 70 MPa to 85 MPa for 8 s to 12 s; a short hold below 5 s produces visible sink marks around the hinge pin bore in production. The material is not intended for direct food contact; the steam valve retainer is separated from food by a stainless steel cover and silicone gasket. If indirect food-contact status is evaluated, the grade must meet FDA 21 CFR 177.1520 olefin polymer migration limits and EU 10/2011 total migration below 10 mg/dm² for the actual part geometry and contact duration. Safety compliance is governed by IEC 60335-2-15:2012 and IEC 60335-1:2020 clause 30.1 ball pressure testing at 125 °C for parts in contact with the outer lid. Final parts include hinge brackets, steam valve retainers, and base housing frames, where cyclic exposure to 100 °C steam followed by cooling to 25 °C over 1,000 cycles is a standard pre-qualification protocol.
When a vacuum cleaner floor nozzle is converted from ABS to Kingfa PP-92010, the mineral filler fraction is held between 12 wt% and 18 wt% to match the flexural stiffness of the former ABS while retaining low-temperature impact after floor contact at -10 °C. The melt temperature is set at 220 °C to 240 °C, the mold temperature at 30 °C to 40 °C, and the injection speed at 80 mm/s to 120 mm/s ram speed on a 1,200 kN machine with a 35 mm screw and 20:1 L/D. Hold pressure is set at 50 MPa to 70 MPa, and cushion is maintained at 3 mm to 5 mm to stabilize packing in a two-cavity family mold. The tool is gated with a fan gate at the nozzle throat, not a pin gate at the brush slot, to prevent jetting along the bottom plate. Because the part is subject to repeated impact on thresholds, impact testing is performed under ISO 180:2019 Izod notched at 23 °C and -10 °C; a drop test from 1 m onto concrete according to the OEM’s internal specification is also common. Electrical safety compliance is under IEC 60335-2-2:2009 for vacuum cleaners, and the plastic floor nozzle is not considered a live part; UL 94 HB is accepted unless the motor is adjacent to the nozzle in a handheld design. Final parts include floor nozzle bodies, brush carrier brackets, and handle locks. Published data for this specific replacement configuration is limited, so OEMs should compare molded plaque properties under ISO 178 and ISO 180 across three production batches before tool approval.
Competitive Kingfa PP-92010,PP Copolymer,Home Appliance, Mineral Filled prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8615365186327 or mail to sales3@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8615365186327
Email: sales3@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Kingfa PP-92010 is a mineral-filled polypropylene copolymer compounded for injection-molded structural and non-appearance home appliance components in which low warpage, moderate stiffness, and chemical resistance are among the controlling requirements. The product code PP-92010 identifies a PP copolymer base resin carrying a dispersed mineral filler, typically talc or a talc/calcium carbonate system for appliance grades, at a loading that is declared on the lot certificate but commonly falls in the 15–25 wt% class for this product family. Because filler content directly alters density, flow, impact, and thermal response, the grade must be evaluated against end-use specifications rather than unfilled PP data.
Representative published property windows for mineral-filled PP copolymer appliance compounds of this class include a density of 1.03–1.08 g/cm³ under ISO 1183-1, a melt mass-flow rate of 8–20 g/10 min at 230 °C and 2.16 kg under ISO 1133-1:2022, a tensile yield strength of 24–30 MPa under ISO 527-2, a flexural modulus of 2000–2800 MPa under ISO 178, a notched Charpy impact energy of 3–6 kJ/m² under ISO 179-1/1eA, and a heat deflection temperature of 100–115 °C at 0.45 MPa under ISO 75-2/B. Published data for the specific PP-92010 configuration is limited; the current Kingfa certificate of analysis controls all lot-specific approvals.
The mineral filler raises apparent melt viscosity and reduces mold shrinkage through plate-like filler morphology. Capillary rheometry on 20 wt% talc-filled PP copolymer grades at 230 °C commonly records an apparent shear viscosity near 90–150 Pa·s at 1000 s⁻¹, compared with 40–70 Pa·s for unfilled PP impact copolymer under equivalent shear rate. The practical consequence is that PP-92010 should not be processed with the melt-pressure limits used for unfilled PP; injection machines operating with 30–40 mm screw diameters and 22–25:1 L/D ratios may show a 15–25% increase in screw torque at the same setpoint.
Mold shrinkage is anisotropic. Published tool-design data for talc-filled PP copolymer report parallel shrinkage of 0.8–1.2% and perpendicular shrinkage of 1.0–1.4% under ISO 294-4, whereas unfilled PP impact copolymer typically exhibits 1.2–2.0% in both axes. The difference between flow and cross-flow shrinkage of 0.1–0.3% must be corrected in core and cavity dimensions to prevent out-of-roundness in circular bosses and bearing bores.
Because talc-filled PP copolymer can adsorb surface moisture at relative humidity above 60%, pre-drying at 80–90 °C for 2–4 h in a desiccant dryer with air dew point below -20 °C is required before molding to prevent splay. On 1200–1600 kN clamp force injection machines with 30–40 mm screws, skipped drying has been observed to produce intermittent silver streaks on textured surfaces at wall stock below 2.0 mm; raising melt temperature alone does not remove the defect because water vapor migrates with the melt front rather than dissolving into the polymer. Lot-specific moisture content should be checked by Karl Fischer titration or weight-loss at 105 °C; a moisture content below 0.10 wt% is commonly specified before molding to avoid splay and surface degradation.
Injection molding of PP-92010 is best performed with a general-purpose or wear-resistant screw having a compression ratio of 2.2–2.8:1, a check-ring valve, and a nozzle orifice of 3–5 mm. Barrel zones are commonly set from hopper to nozzle as 180 °C, 200 °C, 215 °C, 225 °C, and 230 °C; melt temperature should be maintained between 210 °C and 240 °C. Residence time above 250 °C should be limited to less than 5 min because the mineral filler and copolymer phase can undergo thermo-oxidative degradation, producing surface chalking and loss of impact.
Mold temperature influences surface replication and impact retention. A mold temperature of 30–60 °C is standard for non-appearance structural parts; textured surfaces benefit from the upper end of this range to prevent gloss mottling. Crystallization temperature of talc-filled PP copolymer is commonly between 120 °C and 128 °C under ISO 11357-3, and rapid cooling below 30 °C can quench the ethylene-propylene copolymer phase, reducing notched impact energy at the gate region.
Table 1 compares class-level property windows for mineral-filled PP copolymer, unfilled PP impact copolymer, and general-purpose ABS. The values are drawn from published technical data sheets and are not lot-specific for PP-92010.
| Property | Test standard | Mineral-filled PP copolymer appliance range | Unfilled PP impact copolymer | General-purpose ABS |
|---|---|---|---|---|
| Density | ISO 1183-1 | 1.03–1.08 g/cm³ | 0.90–0.91 g/cm³ | 1.03–1.07 g/cm³ |
| Tensile yield strength | ISO 527-2 | 24–30 MPa | 22–28 MPa | 35–45 MPa |
| Flexural modulus | ISO 178 | 2000–2800 MPa | 900–1300 MPa | 1900–2400 MPa |
| Notched Charpy impact | ISO 179-1/1eA | 3–6 kJ/m² | 10–20 kJ/m² | 15–30 kJ/m² |
| HDT at 0.45 MPa | ISO 75-2/B | 100–115 °C | 85–95 °C | 90–100 °C |
| Mold shrinkage, parallel | ISO 294-4 | 0.8–1.2% | 1.2–2.0% | 0.4–0.8% |
| Coefficient of linear thermal expansion | ISO 11359-2 | 50–80 µm/m·°C | 100–150 µm/m·°C | 80–110 µm/m·°C |
Table 1 shows that the PP-92010 class is positioned between unfilled PP and ABS in flexural modulus and mold shrinkage, but its notched impact energy is lower than both unfilled PP and ABS. The data should not be used for finite-element analysis input without conducting tensile and creep tests on the actual lot because filler content, particle size distribution, and coupling-agent package can shift flexural modulus by ±300 MPa and notched impact by ±1.5 kJ/m².
On twin-screw compounding lines with 40:1 L/D, mineral filler is often side-fed after the melting zone to preserve platelet aspect ratio and reduce barrel wear. Direct hopper feeding of talc can increase screw and barrel wear in the feed zone; nitrided or bimetallic barrels are specified when filler loading exceeds 20 wt%. For injection molders, filler content above 25 wt% can produce gate blush and jetting if the gate shear rate exceeds 10,000 s⁻¹; gate dimensions should be established by capillary rheometry and short-shot studies under ISO 294-1 rather than by trial-based adjustment.
In washer and dishwasher structural brackets, PP-92010 is typically selected because the talc filler reduces post-mold warpage in flat sections with wall-thickness transitions from 2.0 mm to 3.5 mm. On a production line with a 40 mm screw and 1600 kN clamp, a melt cushion of 3–6 mm and screw decompression of 3–5 mm have been used to prevent nozzle drool from the higher-viscosity mineral-filled melt. Gate land length should be 0.5–1.0 mm, and gate thickness should be at least 60% of the part wall to prevent jetting because the filled melt exhibits shorter flow length than unfilled PP at equal injection pressure.
Against unfilled PP impact copolymer, PP-92010 increases flexural modulus by approximately 50–100% and reduces mold shrinkage by 0.4–0.9% absolute. The trade-off is lower notched impact energy, typically 3–6 kJ/m² compared with 10–20 kJ/m² for unfilled impact copolymer. The mineral filler also raises density from 0.90–0.91 g/cm³ to 1.03–1.08 g/cm³, which increases part weight and may require adjustment of wall thickness or rib geometry.
Against general-purpose ABS, PP-92010 offers a different profile. Both materials occupy a similar density range, but mineral-filled PP copolymer typically processes at lower melt temperature, 210–240 °C versus 220–260 °C for ABS, and shows lower mass change under ISO 175 immersion in 5% sodium hydroxide at 60 °C, which is relevant in dishwasher and washing machine environments. However, ABS generally provides higher notched impact energy, 15–30 kJ/m², higher tensile yield strength, 35–45 MPa, lower mold shrinkage, 0.4–0.8%, and better paint adhesion without flame or plasma pretreatment. PP-92010 is therefore not a direct aesthetic replacement for ABS unless the part function and surface treatment chain are revalidated. Within the broader PP compound portfolio, glass-fiber-filled PP offers higher flexural modulus, typically 3500–5000 MPa under ISO 178, but mineral-filled PP-92010 offers lower density, lower anisotropy, and lower abrasion on injection barrels.
The increase in heat deflection temperature to 100–115 °C is caused by filler rigidity and higher crystallinity; however, Vicat softening temperature under ISO 306 Method A50 for this class is typically 145–155 °C, and it may not correlate with load-bearing temperature. Structural parts subjected to continuous stress above 70 °C should be evaluated for creep because talc-filled PP can show non-linear strain accumulation under sustained load, especially in washing machine spin tubs. Creep modulus after 1000 h at 60 °C for 20 wt% talc-filled PP is generally 1000–1500 MPa; published data for PP-92010 specific configuration is limited.
Appliance enclosures and structural components must be evaluated in the final part geometry. Talc-filled PP copolymer compounds of this class are commonly classified UL 94 HB at 3.0 mm thickness under IEC 60695-11-10; the current UL Yellow Card for Kingfa PP-92010 controls the classification. For components in unattended appliances, glow-wire testing under IEC 60695-2-11 is applied at 750 °C or 850 °C depending on connection current and isolation, according to IEC 60335-1 clause 30.2. Because mineral-filled PP is not inherently glow-wire ignition resistant at 750 °C, part thickness, rib density, and melt residence history can affect pass/fail performance.
Substance compliance for Kingfa PP-92010 should be confirmed through supplier declaration against RoHS 2011/65/EU with lead content ≤0.1 wt%, cadmium ≤0.01 wt%, mercury ≤0.1 wt%, hexavalent chromium ≤0.1 wt%, and PBB/PBDE ≤0.1 wt%. REACH obligations under EU 1907/2006 Article 33 apply if candidate list substances exceed 0.1 wt% at article level. The polypropylene polymer matrix falls under FDA 21 CFR 177.1520; however, mineral fillers and additive packages require separate conformity review for food-contact use, which is not normally the end-use for PP-92010 home appliance components.
| Compliance domain | Standard | Typical evaluation condition |
|---|---|---|
| Flammability | UL 94 HB / IEC 60695-11-10 | 3.0 mm thickness; final Yellow Card controls |
| Glow-wire ignition and flammability | IEC 60695-2-11 | 750 °C or 850 °C for unattended enclosures under IEC 60335-1 |
| RoHS restricted substances | RoHS 2011/65/EU | Pb ≤0.1 wt%, Cd ≤0.01 wt%, Hg ≤0.1 wt%, Cr(VI) ≤0.1 wt%, PBB/PBDE ≤0.1 wt% |
| REACH SVHC | EU 1907/2006 Article 33 | Declaration below 0.1 wt% at article level |
| Food-contact polymer matrix | FDA 21 CFR 177.1520 | Only where finished article is cleared; fillers require separate review |
For production qualification, PP-92010 should be tested on the intended injection machine using a mold with pressure sensors at the gate and end-of-fill. Short-shot studies under ISO 294-1 are used to establish the lower pressure boundary, and gate-seal time is determined from part weight stabilization with hold-pressure time. Because published data for this specific configuration is limited, lot-specific rheology and filler content certificates from Kingfa are required before tool steel is cut.