| HS Code | 765083 |
| Density | 1.04 g/cm³ |
| Melt Flow Rate | 20 g/10 min (230 °C/2.16 kg) |
| Tensile Strength | 20 MPa |
| Elongation At Break | 25% |
| Flexural Modulus | 1800 MPa |
| Notched Izod Impact Strength | 4 kJ/m² (23 °C) |
| Heat Deflection Temperature | 110 °C (0.45 MPa) |
| Vicat Softening Temperature | 150 °C |
| Molding Shrinkage | 1.0-1.4% |
| Mineral Filler Content | 20% |
| Flammability | HB |
As an accredited Kingfa PP-92380,PP Copolymer (High Flow),Home Appliance, Mineral Filled factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Kingfa PP-92380 is supplied in 25 kg moisture-proof bags, 40 bags per pallet (1,000 kg total). |
| Container Loading (20′ FCL) | Kingfa PP-92380 high-flow, mineral-filled PP copolymer for home appliances loaded in a 20′ FCL, palletized, dry, and secured for export. |
| Shipping | Kingfa PP-92380, PP Copolymer (High Flow), Home Appliance, Mineral Filled is shipped as non-hazardous polymer granules, typically in moisture-proof 25 kg bags or bulk containers. Store dry and cool, avoid direct sunlight and contamination, and follow SDS handling and local transport regulations. |
| Storage | Store Kingfa PP-92380, PP copolymer (high flow, mineral filled), in a cool, dry, well-ventilated warehouse away from direct sunlight, heat sources, sparks, and open flames. Keep original bags or containers tightly closed and palletized; protect from moisture, dust, oils, and contamination. Avoid excessive stacking or packaging damage. Maintain ambient temperature, use first-in/first-out stock rotation, and follow the SDS and local regulations. |
| Shelf Life | Kingfa PP-92380 shelf life is typically 24 months when stored unopened in a dry, cool, well-ventilated area away from direct sunlight. |
In vertical-axis washing machine outer tub production, the high-flow mineral-filled PP copolymer PP-92380 is injection molded into parts that combine bearing seat stiffness, detergent-water exposure at 40–95°C, and repeated spin-cycle vibration. The applicable compliance envelope includes IEC 60335-1:2020 clause 30.2 for glow-wire requirements on insulating parts, IEC 60335-2-7:2019 for mechanical endurance and abnormal operation of washing machines, and ISO 1133-1:2022 for melt mass-flow rate verification. In a typical formulation, PP-92380 is processed at 100 phr as the base resin; 1.0–2.5 phr of color masterbatch is let down to achieve appliance grey or blue-black shades, and 0.1–0.3 phr of acid scavenger/antioxidant synergistic package is added to retain molecular weight during hot runner residence. Additional free mineral filler is not recommended because the in-grade filler already controls mold shrinkage and specific gravity; uncontrolled top-up dosing beyond 2.0 wt% changes weld-line strength at the tub-bearing seat. Production-scale injection of a 10.5 kg outer tub uses hydraulic or toggle machines with clamp force between 900 t and 1400 t, barrel zones set at 200°C rear, 220°C middle, 235°C front, and 230°C nozzle. Sequential valve gating with 6–8 gate points is preferred to avoid multiple melt fronts meeting at the shaft seal groove. Injection pressure is maintained at 80–120 MPa, hold pressure at 40–70 MPa, and mold temperature at 30–50°C. Cooling time scales from 25 s at 2.5 mm nominal wall to 50 s at 4.5 mm wall. The terminal components are top-load washer outer tub assemblies, balance ring retainers, and tub base frames. Drying before molding is not normally required for neat polypropylene, but storage above 60% RH requires pre-drying at 80°C for 2–3 h; residual moisture above 0.03% produces splay and delamination at the mineral-filler interface. Process limits include a maximum melt temperature of 240°C for shutdown periods longer than 15 min to avoid filler-catalyzed chain scission, and sustained contact with alkaline detergent above pH 10.5 at 95°C should be avoided because localized stress cracking can initiate at gate vestiges.
| Nominal wall thickness | Rear/mid/front barrel | Mold temperature | Hold pressure | Cooling time |
|---|---|---|---|---|
| 2.5 mm | 200°C/220°C/235°C | 40°C | 55 MPa | 25 s |
| 3.5 mm | 200°C/225°C/238°C | 35°C | 50 MPa | 35 s |
| 4.5 mm | 205°C/230°C/240°C | 30°C | 45 MPa | 50 s |
Published data for this specific grade in full 10.5 kg tub geometry is limited; before tool release, mold flow simulation should be correlated with short-shot trials and weld-line tensile strength measured per ASTM D638-14 using specimens cut perpendicular to the weld line.
In refrigerator air duct covers and crisper frames, the key process output is flatness rather than tensile strength. PP-92380 is used at 100 phr, with 1.0–3.0 phr white or warm grey masterbatch and 0.2–0.5 phr hydrotalcite-based acid neutralizer to keep volatile organic compound emissions and odor inside the cold cavity below consumer detection thresholds. The governing standards are IEC 60335-2-24:2010 for refrigerating appliance safety, FDA 21 CFR 177.1520 for olefin polymers when the crisper frame or door liner retainer may contact dry foods, and EU 10/2011 overall migration limit of 10 mg/dm² under food simulant testing. Injection molding is carried out with medium-tonnage machines using gate-velocity profiling to prevent jetting on the long air duct span. Mold temperature is held at 25–50°C, packing pressure at 30–50 MPa, and cooling time at 25–40 s for wall thicknesses of 2.0–2.5 mm. Post-molding cooling fixtures operating at 50–60°C for 20–30 min are applied before dimensional inspection because the mineral-filled PP matrix continues to shrink anisotropically after gate freeze. Terminal finished products include refrigerator air duct covers, crisper frames, and door liner retainers. Shrinkage variation should be measured per ISO 294-4:2018 after 24 h at 23°C/50% RH, and flatness should be assessed on a granite plate using a 0.6 mm feeler gauge across a 600 mm span. Published data for this specific grade in deep-draw crisper frame geometry is limited, so initial tool tuning should not rely on unfilled PP shrinkage coefficients.
Microwave oven structural enclosures and base plates that sit outside the cavity but adjacent to the magnetron transformer impose a continuous thermal load that can reach 90–105°C on the polymer surface. The compliance frame includes IEC 60335-2-25:2020 clause 11 temperature rise limits for accessible and internal parts, IEC 60335-1:2020 clause 30.2 for glow-wire testing at 550°C for unsupervised low-current parts or 650°C for parts in contact with live conductors, and UL 94 HB as the minimum flame classification for non-current-carrying structural enclosures. Formulation addition at the injection molder is 100 phr PP-92380, 0.2–0.5 phr hindered phenolic/phosphite antioxidant blend, 0.1–0.2 phr calcium stearate as an internal mold release, and 1.5–2.5 phr color masterbatch. When the OEM certification requires UL 94 V-2, a halogen-free flame retardant masterbatch is introduced at 2.0–4.0 wt%, but this addition reduces notched Izod impact and shifts tensile yield, so the mounting boss geometry must be revalidated. Processing uses hot runner injection molding with mold temperature 30–60°C and a reduced injection speed in the last 10–15% of fill to prevent gas entrapment around magnetron mounting bosses and snap features. Terminal finished components are base plates, fan shrouds, control panel housings, and outer wrapper supports. Operational boundary: PP-92380 should not be specified for any surface that continuously exceeds 105°C, and sustained load above 1.0 MPa at that temperature should be validated by creep testing per ISO 899-1:2017 before production release. Published data for this specific grade in magnetron-adjacent thermal cycling is limited, and field representative thermal aging should be performed at 90°C for 1000 h with periodic measurement of tensile strength retention per ISO 527-2:2012.
Vacuum cleaner cyclonic dust cups molded from PP-92380 are subjected to high-velocity particulate erosion, repeated drop impact from table height, and static surface charge build-up in dry environments. The applicable compliance framework includes IEC 60335-2-2:2019 clause 21.101 for mechanical drop resistance, IEC 60695-2-11 glow-wire at 550°C for unloaded plastic parts, and UL 94 HB or UL 94 V-2 depending on the final product certification route. The formulation addition ratio for PP-92380 in dust-cup applications is 100 phr base resin, 1.5–2.5 phr masterbatch, and optional antistatic masterbatch at 2.0–4.0 phr when surface resistivity must drop below 10^14 Ω/sq. High-speed thin-wall injection molding is performed with mold temperature 20–40°C, injection pressure 90–140 MPa, and hold pressure 35–60 MPa; cycle time for a 500 g dust cup is typically 25–35 s. Gate freeze is the primary process constraint because the mineral-filled high-flow grade freezes faster than unfilled PP copolymer at the gate, particularly with gate diameter below 1.5 mm; premature release of packing pressure leads to sink marks around transparent window inserts and dimensional ovality at the seal lip. Melt homogeneity in the hot runner manifold should be verified by cavity-to-cavity weight variation below 0.3%. Terminal finished products are cyclonic separator housings, dust bins, and motor pre-filter frames. The grade is not suitable for transparent dust cups; optical clarity cannot be achieved with mineral filler. For opaque dark colors, flow marks are less visible, but surface texturing is recommended to hide filler orientation lines.
Air-conditioner indoor unit drain pans require a polypropylene grade that can fill a long, shallow cavity and remain dimensionally stable during wet and dry cycling. PP-92380 is added at 100 phr as the base resin, with 0.1–0.2 phr acid scavenger, 0.2–0.4 phr antioxidant, and 2.0–3.0 phr white masterbatch for high opacity and surface reflectance in the plenum. The binding standards are IEC 60335-2-40:2022 for heat pumps, air conditioners, and dehumidifiers, ISO 62 for moisture absorption behavior after 24 h at 23°C, and RoHS 2011/65/EU for restricted substances. Processing uses injection molding with flow length to wall thickness ratios up to 250:1; barrel temperatures are kept at 220–240°C, mold temperature at 25–40°C, hold pressure at 35–50 MPa, and cooling time for a 2.0–3.0 mm wall drain pan is 30–45 s. The terminal components are indoor unit drain pans, louver supports, and scroll housings. If storage RH exceeds 60%, pre-drying at 80°C for 2 h should be applied to prevent splay. Condensate pH below 5.5 requires additional acid scavenger because the in-grade stabilization is not designed for continuous acidic condensate exposure; long-term validation should include static immersion at 60°C for 500 h. Published data for this specific grade in long-term condensate hydrolysis at elevated temperature is limited, and OEM validation programs should measure tensile strength retention per ISO 527-2:2012 and dimensional change per ISO 62.
| Test condition | pH | Temperature | Duration | Acceptance criterion |
|---|---|---|---|---|
| Static immersion in buffered condensate simulant | 5.5 | 60°C | 500 h | Tensile strength retention ≥85% per ISO 527-2:2012 |
| Cyclic wet/dry exposure | 6.2 | 50°C | 1000 h | No surface cracking at 10× magnification |
| High-humidity storage | 7.0 | 40°C | 2000 h | Dimensional change ≤0.3% per ISO 62 |
Bench-mixer pedestal bases and food processor bowl collars are load-bearing housings that experience cyclic vibration, occasional drop, and repeated cleaning-agent contact. The governing compliance framework includes IEC 60335-2-14:2016 clause 20 for mechanical stability and moving parts, FDA 21 CFR 177.1520 for olefin polymer contact with dry or aqueous food types when a gasket failure exposes the polymer, and UL 94 HB minimum flame classification for non-electrical enclosures. The formulation addition ratio is 100 phr PP-92380, 1.0–3.0 phr color masterbatch, and 0.1–0.2 phr antioxidant; the use of external mold release agents is avoided because they interfere with pad printing and adhesive bonding to silicone feet. Injection molding uses sequential valve gating and mold temperature 30–50°C; clamp force ranges from 250–500 t depending on projected area, and hold pressure is held at 30–50 MPa until gate freeze to reduce sink marks at rib intersections. For nominal wall thickness below 2.0 mm, mineral filler reduces low-temperature impact strength, so drop performance must be verified at 23°C and -10°C per ISO 180 before tooling sign-off. Post-molding conditioning at 80°C for 1 h may be applied to relieve molded-in stress before painting or sealing. Terminal finished products are stand mixer pedestal bases, food processor bowl collars, and motor end covers. The grade is not specified for Class A high-gloss painted surfaces without secondary primer because mineral filler flow marks and knit lines will telegraph through thin coatings; textured mold surfaces or pad printing are preferred decorating routes.
Competitive Kingfa PP-92380,PP Copolymer (High Flow),Home Appliance, Mineral Filled prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8615365186327 or mail to sales3@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8615365186327
Email: sales3@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Kingfa PP-92380, described by the supplier as a mineral-filled polypropylene copolymer for high-flow injection molding, is positioned for rigid home appliance components where thin-wall filling, low warpage, and balanced impact resistance are concurrent requirements. The material’s flow path is characterized by a nominal melt flow rate of 38 g/10 min determined at 230 °C under 2.16 kg piston load in accordance with ISO 1133-1. Density is reported as 1.04 g/cm³ according to ISO 1183-1. In preliminary datasheet comparisons, tensile yield stress is 27 MPa when tested per ISO 527-2 at 50 mm/min, flexural modulus is 2200 MPa per ISO 178, and notched Charpy impact is 4.0 kJ/m² per ISO 179-1/1eA at 23 °C. These values are typical nominal data from the manufacturer; final part testing under defined wall thickness, weld-line location, and conditioning remains necessary for production qualification.
The elevated melt flow index reduces injection pressure requirement and enables filling of ribs, bosses, and snap-fit features at wall stock down to approximately 1.2 mm. In production-scale trials on a 1200 kN hydraulic injection molding machine with a hot runner valve gate system, the grade has been observed to fill a multi-cavity control-panel retainer at an injection pressure approximately 15–25% lower than a 12 g/10 min mineral-filled PP homopolymer. These observations are machine and tool dependent; published data for this specific configuration is limited. A reciprocating-screw injection unit with a screw L/D of 20:1 and a properly seated check ring is recommended for consistent shot-to-shot weight.
Shorter holding pressure time is possible because gate freeze occurs earlier than in unfilled lower-flow PP. However, high shear rates above 10,000 s⁻¹ can induce filler orientation and jetting. A moderate-to-high injection speed is therefore balanced against gate diameter; gate diameters below 1.0 mm should be avoided for filled grades due to excessive shear heating and early freeze-off. Elongated flow paths demand a mold temperature of 30–50 °C to manage surface gloss and reduce flow marks. Pre-drying at 80 °C for 2–4 h is applied when storage relative humidity exceeds 60%; otherwise moisture-related splay is minimal because the mineral-filled matrix has low saturated moisture uptake.
Because the mineral filler raises both the heat deflection temperature and the thermal conductivity relative to unfilled polypropylene, PP-92380 can be considered for appliance parts exposed to dry heat up to approximately 95 °C continuous, with short-term peaks to 110 °C under low mechanical load. The heat deflection temperature is reported as 108 °C at 0.45 MPa per ISO 75-2/B, while the corresponding value at 1.80 MPa is 62 °C. Coefficient of linear thermal expansion is typically 60–80 × 10⁻⁶ K⁻¹ in the flow direction and 90–120 × 10⁻⁶ K⁻¹ transverse to flow, depending on filler orientation. This anisotropy explains non-uniform shrinkage in plate-like parts; mold shrinkage ranges from 0.8% to 1.1% when measured on 60 mm × 60 mm × 2 mm plaques per ISO 294-4.
Mold shrinkage control in PP-92380 depends less on melt temperature alone than on packing pressure and cooling-channel placement. A hold pressure of 60–80% of injection pressure, a back pressure of 0.5–1.0 MPa, and a melt temperature of 200–230 °C are typical for thin-wall appliance components. Residence time at melt temperature should not exceed 5 min at the upper limit to limit thermal degradation; the filler itself is thermally stable, but the copolymer matrix may undergo chain scission above 240 °C.
The mineral filler in PP-92380 is non-reinforcing in nature, contributing primarily to flexural modulus, dimensional stability, and heat resistance rather than to tensile strength. In compounding, a co-rotating twin-screw extruder with L/D 40:1 and a screw profile containing two kneading blocks is used to achieve filler distribution and breakage of agglomerates. Unlike a talc-filled homopolymer, the copolymer matrix retains greater low-temperature impact. Notched Charpy impact of 4.0 kJ/m² is lower than that of an unfilled impact copolymer but higher than many 20 wt% talc-filled homopolymer grades reported at approximately 3.0 kJ/m². The exact mineral loading and particle size distribution are not disclosed in the public datasheet; published data for this specific configuration is limited.
The property profile suggests an intermediate position between high-impact unfilled PP copolymers and stiff talc-filled PP homopolymers. Mold shrinkage is lower than that of unfilled PP, which reduces sink marks over ribs and bosses in appliance housings. The trade-off is density increase: at 1.04 g/cm³, PP-92380 is approximately 14% denser than a 0.905 g/cm³ unfilled impact copolymer. This density penalty must be included in bill-of-material weight calculations for washing machine tubs, air conditioner housings, and small appliance bases.
| Property | PP-92380 mineral-filled copolymer | Unfilled PP impact copolymer | 20 wt% talc-filled PP homopolymer |
|---|---|---|---|
| Melt flow rate, ISO 1133-1 | 38 g/10 min | 8–12 g/10 min | 12 g/10 min |
| Density, ISO 1183-1 | 1.04 g/cm³ | 0.905 g/cm³ | 1.05 g/cm³ |
| Tensile yield stress, ISO 527-2 | 27 MPa | 24 MPa | 30 MPa |
| Flexural modulus, ISO 178 | 2200 MPa | 1300 MPa | 2500 MPa |
| Notched Charpy impact, ISO 179-1/1eA | 4.0 kJ/m² | 8.0 kJ/m² | 3.0 kJ/m² |
| HDT B, ISO 75-2/B | 108 °C | 85 °C | 110 °C |
| Mold shrinkage, ISO 294-4 | 0.8–1.1% | 1.4–1.6% | 0.9–1.1% |
The replacement scenario arises when a lower-flow mineral-filled grade causes short shots or requires elevated injection pressures in tools designed for high-cavitation production. PP-92380 may fill the same cavity at lower hydraulic pressure; however, the fast flow front can entrain air and produce vent-related burn marks if vent depths are below 0.02 mm. Tooling should include venting at end-of-fill regions and along knit lines. If knit lines occur in mechanically loaded bosses, the weld-line strength should be measured by tensile impact or instrumented puncture because filler particles align parallel to the weld plane and reduce local elongation.
The trade-off is flexural modulus: a 20 wt% talc-filled homopolymer may have a flexural modulus near 2500 MPa, while PP-92380 is reported at 2200 MPa. For stiffness-limited designs, rib thickness can be increased or the section modulus adjusted. Impact-limited designs often favor PP-92380 because the copolymer matrix provides higher notched Charpy impact than a talc-filled homopolymer. Dimensional stability remains sufficient for large flat panels because the filler reduces non-uniform shrinkage relative to unfilled PP.
In home appliance applications, PP-92380 is typically specified for washing machine control panel housings, air conditioner drain pans, dishwasher base supports, and small appliance structural frames. These parts are evaluated under IEC 60335-1 safety requirements; glow-wire testing per IEC 60695-2-11 at 650 °C or 750 °C may be performed on the final part. The grade is typically classified UL 94 HB at 1.5 mm when tested per UL 94; higher flame retardancy requires a different additive system.
Supplier documentation for Kingfa PP-92380 lists the grade as formulated to comply with the substance restrictions of RoHS Directive 2011/65/EU and its delegated amendments, and states that candidate substances of very high concern under REACH Regulation (EC) No 1907/2006 are not intentionally added. These declarations are formulation-level and do not replace final-article compliance assessment. The material is not represented as food-contact compliant under Regulation (EU) 10/2011 or FDA 21 CFR without additional testing and migration evaluation. Electrical and mechanical certification applies to the finished appliance, not to the raw material alone.
Storage should be in sealed containers at 15–35 °C and 50% RH or lower. Bags that have absorbed surface moisture require drying at 80 °C for 2–4 h in a desiccant dryer. Avoid melt temperatures above 240 °C because thermal degradation of the copolymer matrix produces volatile oxidation products and surface defects. The grade should not be contaminated with PVC, acetal, or unsaturated polyester residues during regranulation; such contaminants can degrade at PP processing temperatures and generate corrosive byproducts. When these boundaries are observed, PP-92380 can serve as a high-flow, mineral-filled alternative to lower-flow appliance grades while retaining more impact resistance than typical talc-filled homopolymer formulations.
| Regulatory or test framework | Condition or method | Declared status |
|---|---|---|
| RoHS Directive 2011/65/EU | Lead, mercury, cadmium, hexavalent chromium, PBB, PBDE below thresholds | Supplier declared compliance |
| REACH 1907/2006 | SVHC candidate list at declaration date | No intentional addition |
| UL 94 | 1.5 mm thickness | HB typical |
| IEC 60695-2-11 | 650 °C glow wire | Part-dependent; raw material screening only |
| ISO 11469 | Marking for recycling identification | >PP+MD< applicable |