Zhuhai Kingfa Biomaterial Co., Ltd.

Zhuhai Kingfa Biomaterial Co., Ltd.

Zhuhai Kingfa Biomaterial Co., Ltd., a production entity within Kingfa Sci & Tech Co., Ltd., compounds biodegradable polyester systems based on poly(lactic acid) (PLA), poly(butylene adipate-co-terephthalate) (PBAT), poly(butylene succinate) (PBS), and starch-filled PBAT or PLA matrices. The production environment is structured around co-rotating twin-screw extruders with L/D ratios between 40:1 and 52:1 and screw diameters from 65 mm to 92 mm, fitted with gravimetric mass-flow feeders having a stated short-term dosing accuracy of ±0.25% and a side feeder for mineral fillers positioned at approximately 24 D to 28 D from the main feed throat. Desiccant-bed dryers reduce pellet moisture to below 250 ppm for PLA and below 500 ppm for PBAT and PBS; the drying air is supplied at a dew point of -40°C or lower and at an inlet air temperature of 80°C for PLA and 80°C to 90°C for PBAT/PBS. If ambient relative humidity exceeds 60%, residence time in the dryer is increased because polyester pellets re-absorb surface moisture rapidly. PLA surface moisture can rise above 300 ppm within 30 min when exposed to 23°C and 65% relative humidity. The compounder therefore maintains closed conveying lines with dried-air purge from dryer discharge to extruder feed port, preventing humidity ingress that would otherwise cause hydrolytic chain scission, a rise in melt flow rate, and downstream loss of melt strength in blown film or cast film operations. Published data for the exact Zhuhai line configuration is limited, but these operating thresholds are common to industrial polyester compounding lines.

What Limits Melt Strength Retention in PBAT/PLA Blown Film at 35 µm Gauge?

Blown film extrusion of PBAT/PLA blends at target gauge 35 µm is constrained by a narrow melt-temperature window and by the dependence of bubble stability on blend ratio and moisture content. The practical formulation range for PBAT/PLA film on single-screw extruders with L/D 30:1 and spiral mandrel dies of 1.2 mm to 1.8 mm die gap is usually 50:50 wt% to 80:20 wt% PBAT/PLA. Below 50 wt% PBAT, bubble oscillation and melt fracture appear at die temperatures below 175°C. The melt temperature at the die is maintained between 165°C and 185°C; above 195°C, PLA contributes lower molecular weight species through thermal and hydrolytic degradation, and the bubble shows a reduction in melt strength measured as a decrease in hang-time before sag. Capillary rheometry on a 60:40 wt% PBAT/PLA compound at 170°C typically shows apparent shear viscosity in the range 300 Pa·s to 600 Pa·s at a shear rate of 100 s⁻¹. Published data for Zhuhai Kingfa's specific commercial film grade is limited, but this range is representative of PBAT-rich compounds with PLA added to increase modulus. If the bubble is operated at blow-up ratio 2.5:1 to 3.0:1 and frost-line height is maintained below 250 mm, the gauge variation at 35 µm can be held within ±5%. Higher frost lines reduce transverse direction orientation and increase blocking tendency. Process conflicts arise when PLA content exceeds 60 wt%: Elmendorf tear strength measured according to ASTM D1922-15 falls by more than 50% compared with the 50 wt% PLA condition, and the film becomes brittle in the machine direction. This property cliff-edge requires that converters not repurpose the same press settings used for PBAT-rich film; die temperature, frost-line height, and winding tension must be re-optimized after each 10 wt% shift in PLA content because the bubble tension-strain curve changes shape.

Published data for the exact screw configuration at Zhuhai Kingfa is limited; however, compounding of talc-filled PLA on industrial production platforms of the type used at the Zhuhai site proceeds with side-fed talc having median particle size 1.0 µm to 2.5 µm at addition levels from 5 wt% to 20 wt%. The twin-screw configuration employs kneading blocks with 45° forward stagger at the side-feed zone and a downstream vacuum vent at 32 D to 36 D; vacuum level is maintained below 50 mbar to strip lactide and moisture. Torque-based process monitoring on comparable lines reveals that specific mechanical energy input increases from about 0.18 kWh/kg for unfilled PLA to between 0.24 kWh/kg and 0.31 kWh/kg at 20 wt% talc, depending on screw speed. The corresponding melt temperature at the die must not exceed 210°C; at 220°C, PLA molecular weight degradation generates lactide that re-condenses on the pelletizer water bath and creates tacky strand surfaces. The same formulations show a reduction in cold crystallization temperature from about 110°C to 95°C when a transesterification catalyst or an epoxide-based chain extender is present; this shift is detected by differential scanning calorimetry according to ASTM D3418-15. Addition of multifunctional epoxide chain extenders at 0.1 wt% to 0.5 wt% of total compound raises melt strength, but the mixture must not be combined with amine-based additives because aminolysis of ester linkages accelerates molecular weight loss and negates the chain-extension effect.

PropertyPLAPBATPBSTest standard
Density1.24 g/cm³ to 1.26 g/cm³1.25 g/cm³ to 1.27 g/cm³1.20 g/cm³ to 1.27 g/cm³ISO 1183-1:2019
Melt flow rate2 g/10 min to 20 g/10 min at 210°C, 2.16 kg3 g/10 min to 8 g/10 min at 190°C, 2.16 kg5 g/10 min to 30 g/10 min at 190°C, 2.16 kgISO 1133-1:2022
Tensile strength at break48 MPa to 70 MPa20 MPa to 35 MPa30 MPa to 45 MPaISO 527-2:2012, ASTM D638-14
Elongation at break2% to 10%500% to 700%200% to 400%ISO 527-2:2012, ASTM D638-14
Flexural modulus3.0 GPa to 4.0 GPa0.05 GPa to 0.10 GPa0.4 GPa to 0.8 GPaISO 178:2019, ASTM D790-17
Melting range150°C to 160°C115°C to 125°C90°C to 115°CISO 11357-3:2018, ASTM D3418-15
Glass transition55°C to 60°C-30°C to -20°C-30°C to -10°CISO 11357-2:2020, ASTM D3418-15

Thermal Degradation Pathways in PBAT/PLA Blends During Cast Film Extrusion

Cast film extrusion of PBAT/PLA blends introduces a different thermal history than blown film because the melt curtain is quenched on a polished chill roll rather than air-cooled in a bubble. The degradation pathway of PLA in the melt is dominated by random chain scission, intramolecular transesterification to lactide, and hydrolytic chain scission. Hydrolytic scission arises when residual moisture above 250 ppm attacks ester linkages. Published kinetic studies report apparent activation energies for PLA thermal degradation in the range 70 kJ/mol to 100 kJ/mol under nitrogen, while hydrolytic degradation in the melt can proceed with an apparent activation energy of 40 kJ/mol to 60 kJ/mol. For PBAT, ester hydrolysis is slower, but terephthalate segments are susceptible to β-scission at temperatures above 250°C. Cast-film melt temperatures are therefore kept below 210°C to suppress both lactide regeneration and PBAT chain scission. The cast film line uses a single-screw extruder with L/D 28:1 to 33:1, a vacuum vent at 20 D to 24 D, and a gear pump before a 1.0 mm to 1.5 mm coat-hanger die. Chill roll temperature is maintained at 15°C to 30°C; for PLA-rich blends above 40 wt% PLA, the roll temperature must be below 25°C to prevent adhesion. The quench rate influences crystallinity: differential scanning calorimetry according to ASTM D3418-15 shows that PLA crystallinity in a 20 µm cast film is often below 5%, and the film remains ductile only if PBAT content is at least 50 wt%. When the same film is annealed at 100°C for 30 min, the PLA phase cold-crystallizes and tensile modulus according to ISO 527-2:2012 increases by more than 30%, but tear resistance measured by ASTM D1004-13 decreases correspondingly.

Injection molding of PBS and PLA/PBS alloys at Zhuhai Kingfa Biomaterial's downstream applications generally uses reciprocating screw machines with screw L/D 20:1 to 24:1, compression ratio 2.5:1 to 3.5:1, and a shut-off nozzle to prevent drool. The compounds are dried to below 250 ppm moisture and fed from a hopper dryer purged with desiccated air at 80°C. Barrel zones are profiled from 160°C at the feed throat to 190°C at the nozzle for PLA-containing compounds. Mold temperature is set between 25°C and 40°C for high-gloss amorphous articles. If the mold is heated to 90°C to 110°C, PLA crystallization occurs and heat deflection temperature under 0.45 MPa according to ISO 75-2:2013 rises from below 55°C to above 90°C, but cycle time lengthens and warpage increases in parts with wall-thickness variation greater than 0.5 mm. Production-scale field data indicate that hold pressure must be kept below 80 MPa for semicrystalline PLA because excessive packing stress at the gate leads to stress whitening in flame-retardant grades; published data for the specific Zhuhai line is limited, but the behavior is consistent with polyester nucleation by talc and poly(D-lactic acid). Residence time should not exceed 5 min at 200°C; longer residence times result in molecular weight loss and a drop in Izod impact strength measured by ASTM D256-10 from 4 kJ/m² to below 3 kJ/m² in PLA/PBS alloys.

When Starch-Filled PBAT Grades Are Extruded at High Throughput on a 75 mm Twin-Screw Line

Starch-filled PBAT compounds produced at high throughput on a 75 mm co-rotating twin-screw extruder with L/D 44:1 and specific torque 11.5 Nm/cm³ require a different screw architecture than PBAT/PLA blends because native starch introduces free moisture and high paste viscosity during gelatinization. The screw uses a first kneading section at 8 D to 10 D for melting PBAT, a second kneading section at 24 D to 28 D for starch dispersion, and two atmospheric vents at 20 D and 32 D before a vacuum port at 36 D. Process temperatures are graded from 120°C at the feed zone to 170°C at the die; increasing die temperature above 180°C accelerates starch caramelization and causes brown specks. The maximum throughput for a 75 mm machine is normally limited by vent flooding rather than torque. At starch loadings above 50 wt%, free water above 5% by weight in the starch feed can produce foaming at the die and thickness surging in sheet extrusion. Melt pressure before the screen changer should not exceed 120 bar; a 250 mm melt filter with screen pack 60/80/100 mesh removes char particles and gel agglomerates. Published data for the actual Zhuhai formulation is limited, but these operational envelopes are used on commercial PBAT/starch lines to prevent vent-flow blockage and to maintain stable pellet production.

Compostability and food-contact compliance of compounds produced by Zhuhai Kingfa Biomaterial are formulation-specific and must be re-verified after addition of masterbatch, filler, or chain extender. Biodegradation testing for packaging is anchored to EN 13432:2000/AC:2005 and ASTM D6400-23, which require a minimum of 90% biodegradation of the organic carbon into carbon dioxide within 180 days under controlled composting conditions, with subsequent disintegration and ecotoxicity evaluation. Heavy-metal content is assessed against the limit values in EN 13432:2000/AC:2005 Annex E, and the test method for aerobic biodegradation is ISO 14855-1:2012. For the European market, REACH registration obligations arise from the monomers and additives present in the compound, not from the compounded article itself; substances of very high concern are screened under Regulation (EC) No 1907/2006 as amended. Food-contact suitability is not automatically conferred by compostability; each grade must be evaluated against Regulation (EU) No 10/2011 and the applicable food-simulant testing protocol for specific migration limits, as well as relevant national legislation. Published data for Zhuhai Kingfa's specific compound formulations in food-contact applications is limited; converters should require migration testing under the intended use temperature and simulant type before commercial use. In addition, compounds containing mineral fillers above 5 wt% require verification of dust generation and melt filtration because agglomerates above 100 µm can reduce dart impact strength measured by ASTM D1709-16a and increase gel count in thin films.

Standard or regulationJurisdictionScopeCore test methodTypical criterion
EN 13432:2000/AC:2005European UnionPackaging recoverable through composting and biodegradationISO 14855-1:2012, ISO 16929:2021, ISO 20200:200490% biodegradation in 180 days; disintegration to <2 mm in 12 weeks; no ecotoxicity
ASTM D6400-23United StatesCompostable plasticsASTM D5338-15, ASTM D6868-2190% carbon-to-carbon dioxide conversion in 180 days
ISO 17088:2021InternationalPlastics — Organic recycling through composting and biodegradationISO 14855-1:2012, ISO 16929:2021Mineralization and disintegration equivalent to EN 13432
Regulation (EC) No 1907/2006European UnionREACH registration and SVHC screeningDossier evaluation by ECHASVHC content below 0.1% w/w in article if applicable
Regulation (EU) No 10/2011European UnionPlastic materials and articles in contact with foodSpecific migration testing in simulants assigned by intended useOverall migration <10 mg/dm² or 60 mg/kg for food; specific migration limits per monomer/additive

Batch-to-batch variance in melt flow rate is controlled by off-line capillary rheometry after every 50 t production run; the acceptance window for blown film grades is typically ±1.0 g/10 min at 190°C and 2.16 kg under ISO 1133-1:2022. If the MFR exceeds the upper control limit, the batch is returned to the dryer or blended with virgin material from the same polymerization platform, because PBAT/PLA phase separation can occur when base resins from different suppliers are mixed without compatibilizer. Converters receiving pellets at ambient humidity above 70% must re-dry before processing even if the foil liner remains intact, because internal condensation during ocean freight can raise surface moisture above 1,000 ppm. Storage in direct sunlight for longer than 6 months should be avoided unless the compound contains a UV stabilizer; unstabilized films can lose more than 40% of elongation at break measured by ISO 527-2:2012 due to photo-oxidative chain scission. These operational boundaries define the usable processing envelope for the comparative property windows presented earlier and are required to avoid melt-strength failure, bubble instability, and mold-fouling deposits observed on production lines processing biodegradable polyester compounds.